making consistant small oval cabs

Post here with questions and topics relating to making glass jewelry.

Moderators: Tony Smith, Brad Walker

making consistant small oval cabs

Postby Chelseaglass » Thu Jun 21, 2012 12:15 pm

Without using a mold, how can I obtain consistant almond sized oval/ovoid shapes? I have tried stacking small rectangles but get rounded corner rectangles as a result. No problem obtaining round cabs with the spiral stack method but the oval shapes have been hit or miss--mainly miss.
Chelseaglass
 
Posts: 85
Joined: Sat Jul 18, 2009 10:10 pm

Re: making consistant small oval cabs

Postby Brad Walker » Thu Jun 21, 2012 12:53 pm

I would try firing a few degrees higher than you currently are. If that doesn't work, try nipping off the corners of the rectangles before you fire. But if the rectangles are fairly small, a higher fusing temperature should do the job.

Also, experiment with one layer vs. two (and maybe even three) to see which works best for you.
Brad Walker
Site Admin
 
Posts: 2341
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA

Re: making consistant small oval cabs

Postby Brock » Thu Jun 21, 2012 1:48 pm

Start with oval blanks . . .
Brock
 
Posts: 8407
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Re: making consistant small oval cabs

Postby Chelseaglass » Thu Jun 21, 2012 3:33 pm

Brock,

I was trying to find a quicker way! Thanks--I used to cut small circles for the cabs until I realized the staggered stack and fire method, but will cut shapes for the next batch.

The pieces I am firing are 4-6 layers thick.
Chelseaglass
 
Posts: 85
Joined: Sat Jul 18, 2009 10:10 pm

Re: making consistant small oval cabs

Postby Morganica » Thu Jun 21, 2012 6:05 pm

You can also try cutting elongated diamonds and nip off the extremely angled corners. One thing: Different colors can give different results with the same schedule (unless you just nuke the heck out it). If you're noticing that some colors give a great oval result and others don't, boosting the schedule as Brad describes will probably solve the problem.
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery

"I wrote, therefore I was." (me)
Morganica
 
Posts: 5530
Joined: Mon May 19, 2003 6:19 pm
Location: Portland, OR

Re: making consistant small oval cabs

Postby twin vision glass » Thu Sep 13, 2012 11:25 pm

Make a fused panel of glass the thickness you want. Get it water jet cut . It is PERFECT and will fit into any silver form or setting. Fire Polish if you desire it as well.
Les
twin vision glass
 
Posts: 3626
Joined: Thu Apr 29, 2004 12:55 am
Location: Invermere,B.C. Canada

Re: making consistant small oval cabs

Postby Barry Kaiser » Fri Sep 14, 2012 11:54 am

Another method is to fuse to approximate size and then grind to size and shape. We have a 6 wheel rotary grinder which makes short work of this process.

Barry
Barry Kaiser
 
Posts: 1552
Joined: Mon Jul 25, 2005 6:54 pm
Location: North Carolina

Re: making consistant small oval cabs

Postby Dolores » Fri Sep 14, 2012 3:04 pm

If you need absolute consistancy as well as high volume, get the blanks waterjet cut. What you save in time, angst, and energy more than covers the cost.

DOLORES
Dolores
 
Posts: 1078
Joined: Mon Jul 14, 2003 9:21 pm
Location: Sunny Southern California


Return to Jewelry Making

Who is online

Users browsing this forum: No registered users and 1 guest