I have my fusing schedules down for standard items. I now want to try something different and am having a little trouble nailing it down (pun not intended).
I have some pieces that I have made with straight type lines - triangles or squares. For one piece I have stacked three triangles of COE96 and am trying to have them remain triangles but smooth the edge and melt together slightly.
I have read that the temp to hit is ~ 1100F.
So I have tried the following with little luck:
Rate 400 up to 1000 hold X 8min
Rate AFAP up to 1100 hold X 20Min
Rate 400 to 850 hold X8 min
Rate 400 to 100

Doesnt seem to be doing much. I started with small time frames to no avail. I'm hesitant to increase the temp for fear of excessive "rounding"

Has anyone successfully done something like this that can point me in the right direction.?

Jerry

Valerie Adams
Posts: 587
Joined: Mon Apr 19, 2004 2:49 pm
Location: Santa Rosa, California
Contact:

Re: Jewelry -stick and smooth, not melt

Postby Valerie Adams » Wed Jan 30, 2013 6:44 pm

I've done a little experimenting with six and seven layers of Bullseye 3mm glass but in my kiln had to fire to about 1275-1300° to get them to stick. I don't have the schedule I used handy but I do remember there was gentle rounding (more like softening) of the edges. And, because my kiln wasn't quite level, the stacks leaned a bit.

I don't know Spectrum, but I'm guessing you're not going hot enough.

Morganica
Posts: 1079
Joined: Mon May 19, 2003 6:19 pm
Location: Portland, OR
Contact:

Re: Jewelry -stick and smooth, not melt

Postby Morganica » Wed Jan 30, 2013 7:04 pm

It's not a temperature thing, it's a heatwork thing--not only how long you hold at the process temperature but how long you spent getting to that process temperature. (And of course it's also dependent on the characteristics of your kiln)

400dph to 1000 and then afap up to 1100 doesn't put a lot of heat into those three layers of glass, so you're leaving a lot for the 1100F to do in 20 minutes.

I'm with Valerie; either raise the temperature considerably or go slower and hold for a much longer time at 1100F, or (better still) try a combination of both. Slow down around 1100F to maybe 200dph (or less), get to 1250F and do your 20 minute hold there. Run a couple of test pieces, and adjust accordingly.
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com

"I wrote, therefore I was." (me)

jer99
Posts: 4
Joined: Tue Dec 13, 2011 4:56 pm

Re: Jewelry -stick and smooth, not melt

Postby jer99 » Wed Jan 30, 2013 8:24 pm

Thanks.
I'll give it a bit longer to ramp up, slow it down and go up to about 1350 for about 20 minutes
I'll respond back once I figure this out.

Laurie Spray
Posts: 321
Joined: Sat Dec 17, 2005 10:32 pm
Location: SANTA CRUZ, CALIFORNIA
Contact:

Re: Jewelry -stick and smooth, not melt

Postby Laurie Spray » Sat Feb 02, 2013 1:27 pm

If you have a saw I think the easier way to go is to make a slab the thickness you want the then to cut them up and fire polish. nice flat edges, straight lines!
Just a thought!
Laurie Spray

New website!! Http://bonnydoonfusedglasstools.com
Maker of stainless steel rings,pattern bar formers, pot melt pots, and Bottomless Molds
glass: http://lauriespray.blogspot.com

Kevin Midgley
Posts: 713
Joined: Mon Mar 10, 2003 11:36 am
Location: Tofino, British Columbia, Canada

Re: Jewelry -stick and smooth, not melt

Postby Kevin Midgley » Sat Feb 02, 2013 1:36 pm

Good luck on the sawing when I didn't see a tack fusing annealing schedule in there. :-k

Laurie Spray
Posts: 321
Joined: Sat Dec 17, 2005 10:32 pm
Location: SANTA CRUZ, CALIFORNIA
Contact:

Re: Jewelry -stick and smooth, not melt

Postby Laurie Spray » Sat Feb 02, 2013 1:52 pm

Yes....as Kevin says....make a slab, anneal well and saw!
Laurie Spray

New website!! Http://bonnydoonfusedglasstools.com
Maker of stainless steel rings,pattern bar formers, pot melt pots, and Bottomless Molds
glass: http://lauriespray.blogspot.com

Stephen Richard
Posts: 302
Joined: Sun Jul 06, 2003 4:36 pm
Location: Glasgow, Scotland
Contact:

Re: Jewelry -stick and smooth, not melt

Postby Stephen Richard » Sun Feb 03, 2013 3:43 pm

jer99 wrote:Thanks.
I'll give it a bit longer to ramp up, slow it down and go up to about 1350 for about 20 minutes
I'll respond back once I figure this out.


Why not make a number of observations of the state of the glass from ca 1100F upwards? Then you will see when the glass conforms to your wishes.
Steve Richard
You can view my Blog at: http://verrier-glass.blogspot.com/

Barb R
Posts: 58
Joined: Tue Jul 26, 2005 3:02 pm
Location: Ft. Collins, CO

Re: Jewelry -stick and smooth, not melt

Postby Barb R » Sun Feb 10, 2013 12:35 am

Kevin Midgley wrote:Good luck on the sawing when I didn't see a tack fusing annealing schedule in there. :-k


I agree with Kevin -- Take a look at Spectrum's suggested firing schedules and adjust your annealing holds and ramps to match the appropriate schedule for whatever thickness of glass you have.

http://system96.com/Pages/FiringGuideF.html

Barb

Barry Kaiser
Posts: 286
Joined: Mon Jul 25, 2005 6:54 pm
Location: North Carolina
Contact:

Re: Jewelry -stick and smooth, not melt

Postby Barry Kaiser » Sun Feb 10, 2013 11:35 am

Okay, I will jump in here with a totally different look at the problem.
First, since this is in the Jewelry section, I am assuming that the pieces are small (less than 2x2 inches)
Schedule:
AFAP to 1050°F hold 20
80 DPM to 1250 hold 25
AFAP to (top temp) hold 12
Off-Done (We crash to 900 twice) then close and wait until temp is 300°F

Top temp depends on the kiln and the type of glass. For our 8x8 the temp is 1420
For our 15x15, top temp is 1360.
We use Bullseye, so top temps can come down about 20 for Spectrum.

jer99
Posts: 4
Joined: Tue Dec 13, 2011 4:56 pm

Re: Jewelry -stick and smooth, not melt

Postby jer99 » Tue Feb 26, 2013 11:11 am

This schedule worked out pretty well, I'm still experimenting:
200 degrees to 1000 hold X 30
100 degrees to 1300 hold X 20
AFAP to 850 hold X 8
AFAP to 100

Someone mentioned cutting and fire polishing. I have read a bit about fire polishing - how does the schedule look for that typically?


Post Reply

Return to “Jewelry Making”

Who is online

Users browsing this forum: No registered users and 2 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com

cron