Glass paint safe for food
Moderators: Brad Walker, Tony Smith
-
BobbieMatus
- Posts: 50
- Joined: Tue Jul 08, 2003 12:21 am
Glass paint safe for food
Looking for paints that would be safe for food.
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: Glass paint safe for food
Ferro, Summerday series is lead free. Sunshine series has some lead but applied and fired properly, it should meet standards. Worst case is overcoat it with clear flux from the Sunshine series 1-800-245-4951.luvhug wrote:Looking for paints that would be safe for food.
I'm teaching a 3 day workshop with Sunshine series before WGWE at Minnennium Arts Center. Summerday behaves the same so techniques are totally applicable.
Both series are china paints so they are formulated to be used with food.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
BobbieMatus
- Posts: 50
- Joined: Tue Jul 08, 2003 12:21 am
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
@ 1480ºF. I've gotten mixed results at 1420. They are good up into the 1500's as well.luvhug wrote:Your are a little tooooo far for a workshop, clear accross the country. Would love to attend though. What is the firing temperature for the Ferro paint.
BTW there are CA folks coming.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Unique Glass Colors makes paints suitable for food contact. "We offer two different glass color products----the original colors and a lead-free version for use on food serving pieces. " See their web site at http://uniqueglasscolors.com/
Best wishes,
Tom in Texas
Best wishes,
Tom in Texas
-
BobbieMatus
- Posts: 50
- Joined: Tue Jul 08, 2003 12:21 am
-
BobbieMatus
- Posts: 50
- Joined: Tue Jul 08, 2003 12:21 am
Ferro Paint for Bert
I called Ferro, and got a big runner around from them, connected me to several different people. Asked for paint safe for food, color charts, and prices. They faxed me and information sheet for Versicolor Enamels Series 75 CL (formulated without lead) This didn't match what you told me. Anyway no prices, got a list of colors and firing range 1140 to 1180. They don't make it easy for you. Just how do you buy these paints, what sizes do they come in, how much are they.
Has anyone worked with Reusche unleaded, are they safe, they are easier to buy.
Bobbie
Has anyone worked with Reusche unleaded, are they safe, they are easier to buy.
Bobbie
Bobbie, if you are looking for dry chinapaint colors you might try Mr. and Mrs. of Dallas. They sell leadfree colors in 1 dram vials or 1/2 pound or full pound quantities. You will have to mix these with the media of your choice to make the paints you want.
http://www.mrandmrsofdallas.com/Product ... Paints.htm
Best wishes,
Tom in Texas
http://www.mrandmrsofdallas.com/Product ... Paints.htm
Best wishes,
Tom in Texas
-
BobbieMatus
- Posts: 50
- Joined: Tue Jul 08, 2003 12:21 am
paint
thanks Tom, I'll check it out
Bobbie
Bobbie
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
TomTom White wrote:Bobbie, if you are looking for dry chinapaint colors you might try Mr. and Mrs. of Dallas. They sell leadfree colors in 1 dram vials or 1/2 pound or full pound quantities. You will have to mix these with the media of your choice to make the paints you want.
http://www.mrandmrsofdallas.com/Product ... Paints.htm
Best wishes,
Tom in Texas
That was a good resource. Their pound price for china paints cost somewhat less than double what I pay per kilo from Ferro, which still makes Ferro good for me.
However they sell the transparent glass colors. These are hard to get in the USA. If I am guessing right, they are Heraeus enamels. I used to buy from Heraeus but they upped their minimum quantity from 1 kilo to 5 kilos. That priced me out of their ballpark.
Ferro makes the transparent colors in Germany, but they don't export them to the USA. I think Heraeus will export them here. I have a couple of colors that are great. Especially a lemon yellow transparent that is stable right up to fusing temps. It is an incredibly strong color. It will even hold up to being covered with cobalt blue. I thought that it would disappear, but it pretty much turned green.
I believe that the Heraeus and Ferro transparent glass colors are superior to the colors available through Reusche. They are more transparent and more glassy.
Fusemaster also resells these enamels Their prices look similar to Mr & Mrs. I thought that Fusemaster charged more, but a quick look said that they were not far apart. They are board sponsors Click on Fusion HQ.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
BobbieMatus
- Posts: 50
- Joined: Tue Jul 08, 2003 12:21 am
Ferro Paint
Still would like to get the Ferro, but how do you buy them. I want small amounts of each color. They never sent me prices??