I've been holding for 15 minutes.
How long to get rid of the tiny bubbles?
Thanks.
How long do I hold at 1200 to ban bubbles?
Moderators: Brad Walker, Tony Smith
-
Jackie Beckman
- Posts: 475
- Joined: Sun Mar 09, 2003 5:01 pm
- Location: Arizona
- Contact:
I could be wrong Nancy, but from the way your question is worded it sounds as though you are holding on the way down. Could that be? I think that because you said to "get rid of the tiny bubbles" indicating that they already exist. You need to prevent them rather than get rid of them.
The idea is to hold and go slowly between the 1150 - 1250 range on the way up. Imagine laying down contact paper. You place the center down first and work towards the edge to squeeze the bubbles out. Same with the glass. You want the center to touch first and before the edges seal, you need to "squeeze" the bubbles out.
You can do this by going very slowly through the range mentioned and adding a soak for 20 to 30 minutes, depending on the design, you may even want to add two soaks in there. Another way to let the middle down first is by placing chads (chips, brads, beads, balls) around the edge of the piece allowing the center to drop before the sides, thus squeezing the bubbles out the edges before air gets trapped.
Jackie
The idea is to hold and go slowly between the 1150 - 1250 range on the way up. Imagine laying down contact paper. You place the center down first and work towards the edge to squeeze the bubbles out. Same with the glass. You want the center to touch first and before the edges seal, you need to "squeeze" the bubbles out.
You can do this by going very slowly through the range mentioned and adding a soak for 20 to 30 minutes, depending on the design, you may even want to add two soaks in there. Another way to let the middle down first is by placing chads (chips, brads, beads, balls) around the edge of the piece allowing the center to drop before the sides, thus squeezing the bubbles out the edges before air gets trapped.
Jackie
-
Paul Tarlow
- Posts: 344
- Joined: Sun Mar 09, 2003 4:06 pm
- Location: Helios Kiln Glass Studio - Austin
- Contact:
Re: How long do I hold at 1200 to ban bubbles?
To squeeze out bubbles I go from 1050F to 1250F @ 75F/hour. I then hold for 60 minutes at 1250F.Nancy wrote:I've been holding for 15 minutes.
How long to get rid of the tiny bubbles?
Thanks.
That is probably excessive -- but it has been 100% reliable for me.
- Paul
-
Barbara Muth
- Posts: 382
- Joined: Sun Mar 09, 2003 8:10 pm
- Location: Washington DC Metropolitan Area
- Contact: