So, nice piece of Opal glass simply cut in a 10x8 rectangle. Bubble everywhere.
Here is my schedule
DPH-temp-hold
300-1000-10
100-1225-30
200-1250-25
300-1425-10
999-960-60
150-700-5
999-100-done
Little bubbles like pimples Otherwise pretty
Here was the original fuse sched
300-1250-45
300-1450-10
999-960-60
150-700-5
999-100-0
Had same little bubbles so I added slower ramp and another bubble squeeze.
Help
Here is my schedule
DPH-temp-hold
300-1000-10
100-1225-30
200-1250-25
300-1425-10
999-960-60
150-700-5
999-100-done
Little bubbles like pimples Otherwise pretty
Here was the original fuse sched
300-1250-45
300-1450-10
999-960-60
150-700-5
999-100-0
Had same little bubbles so I added slower ramp and another bubble squeeze.
Help
Re: Dang bubbles
A single 3mm piece of glass, or was it two 3mm sheets for 6mm total? If one sheet, that's the problem.
Other than that, was the kiln shelf with kiln wash dry? If not, bubbles.
Do you have a picture of the bubbles? That will help a lot, too.
Change the 300 DPH to 1425 to AFAP to 1425. No reason to go at 300 and chance devit scum. This wont help with the bubbles, just will help overall.
Other than that, was the kiln shelf with kiln wash dry? If not, bubbles.
Do you have a picture of the bubbles? That will help a lot, too.
Change the 300 DPH to 1425 to AFAP to 1425. No reason to go at 300 and chance devit scum. This wont help with the bubbles, just will help overall.
-
Aglassygirl303
- Posts: 47
- Joined: Sun Nov 08, 2009 10:08 pm
Re: Dang bubbles
Standard two pieces of 96coe glass fused together.
Kiln Shelf is a Kaiser Lee Board lined with fresh thin fire paper
I have never had devit, except for when my thermocoupler was sticking inside the kiln wall around 4 inches. But otherwise never.
Kiln Shelf is a Kaiser Lee Board lined with fresh thin fire paper
I have never had devit, except for when my thermocoupler was sticking inside the kiln wall around 4 inches. But otherwise never.
-
Aglassygirl303
- Posts: 47
- Joined: Sun Nov 08, 2009 10:08 pm
Re: Dang bubbles
I tried to post a picture but too big to upload, The glass is perfect and smooth but there are very small bumps, like it has pimples or boils. They are not even but there are many. I seems to happen on the streaky glass or the opals, not on solids. This is new. I have worked many times with both of these glasses. I wonder if my glass dealer is selling "seconds" I do see some pits in the pieces I have not fired yet. Could that be an issue? 
Re: Dang bubbles
You can always send the image to www.imgur.com and then paste the link here....
-
rosanna gusler
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
Re: Dang bubbles
the water in a not dry kiln shelf is way gone before the glass is soft .beninfl wrote:A single 3mm piece of glass, or was it two 3mm sheets for 6mm total? If one sheet, that's the problem.
Other than that, was the kiln shelf with kiln wash dry? If not, bubbles.
Do you have a picture of the bubbles? That will help a lot, too.
Change the 300 DPH to 1425 to AFAP to 1425. No reason to go at 300 and chance devit scum. This wont help with the bubbles, just will help overall.
artist, owner of wanchese art studio, marine finisher
-
JestersBaubles
- Posts: 705
- Joined: Fri Feb 25, 2011 12:01 am
- Location: North Logan, UT
- Contact:
Re: Dang bubbles
Slower ramp from 1000 up to 1225 -- 50 deg/hr.Aglassygirl303 wrote:
Here is my schedule
DPH-temp-hold
300-1000-10
100-1225-30
200-1250-25
300-1425-10
999-960-60
150-700-5
999-100-done
Help
Longer hold at bubble squeeze -- 60 minutes.
I typically ramp to 1100, hold for 30, then ramp to 1225.
2 cents,
Dana W.
-
rosanna gusler
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
Re: Dang bubbles
i like a hold at 1100f as well. things just go better over all if i spend 20 or so min there.
artist, owner of wanchese art studio, marine finisher
-
Aglassygirl303
- Posts: 47
- Joined: Sun Nov 08, 2009 10:08 pm
Re: Dang bubbles
Thank you, I will try that. 
-
DonMcClennen
- Posts: 381
- Joined: Sun Mar 09, 2003 9:09 pm
- Location: Ontario
Re: Dang bubbles
A chad is a little piece of glass, that you use at the edges of the two layers of glass to help air escape during the bubble squeeze. It allows the center of the piece to start to fuse before the side do; as if the sides fuse first, then air, ergo bubbles, get trapped in the middle.
Chads can be a single piece of frit, a piece of stringer, or a piece of scrap. Depending on the placement, you might need to do some coldworking at the end to smooth the edges where the chad was placed, or not.
Other ways, as mentioned above, to get rid of bubble, is a long, long bubble squeeze.
Having said all this, I did some tiles around Christmas for some family gifts; I did a long, long bubble squeeze, and also got pimples, or abcessess, as I called them. I would not call them bubbles, but the glass rose up in certain spots, it didn't look like a bubble as much as it looked like a bad pimple coming to the surface. Someone else suggested to me it might have been the glass (Bullseye Stiff Black).
Hope this helps!
Rachel
imaglassydiva@aol.com
Chads can be a single piece of frit, a piece of stringer, or a piece of scrap. Depending on the placement, you might need to do some coldworking at the end to smooth the edges where the chad was placed, or not.
Other ways, as mentioned above, to get rid of bubble, is a long, long bubble squeeze.
Having said all this, I did some tiles around Christmas for some family gifts; I did a long, long bubble squeeze, and also got pimples, or abcessess, as I called them. I would not call them bubbles, but the glass rose up in certain spots, it didn't look like a bubble as much as it looked like a bad pimple coming to the surface. Someone else suggested to me it might have been the glass (Bullseye Stiff Black).
Hope this helps!
Rachel
imaglassydiva@aol.com
-
Aglassygirl303
- Posts: 47
- Joined: Sun Nov 08, 2009 10:08 pm
Re: Dang bubbles
RachelM, really funny you should mention the glass. I have been fusing for 8 years, always have used Spectrum System 96, that is what I learned on. I have had the same Kiln and used the same schedules for the same sizes and shapes. Suddenly I am getting these bubble?!?!?! Small and larger pieces. It has been making me nuts. So I am looking at the glass last night and there are little pecks all over the surface. I have purchase my glass from the same person for a while too. I have never had any reason to inspect the glass but I may be doing that now. I just wonder if she either received a bad bunch of glass or perhaps she purchase seconds? Is that even possible to get a bad batch of glass?