Postby BobbieMatus » Thu Oct 23, 2003 6:39 am

I have been trying to do two firings a day, slumping bottles. Does anyone have a firing schedule a bit faster then this one
500 to 1100 10 min hold
250 to 1300
full to 1500 5min hold
full to 950 30 min hold

this one works great but takes too long, any suggestions would be helpful
thanks
Bobbie

rosanna gusler
Posts: 730
Joined: Mon Mar 10, 2003 2:22 pm
Location: wanchese north carolina
Contact:

Postby rosanna gusler » Thu Oct 23, 2003 7:18 am

i would go 9999from 1100 to top temp. i would anneal at around 1020 for bottle glass. rosanna

BobbieMatus
Posts: 50
Joined: Tue Jul 08, 2003 12:21 am

Postby BobbieMatus » Thu Oct 23, 2003 7:29 am

thanks, I'll try it
Bobbie

Pat Loboda
Posts: 29
Joined: Tue Mar 11, 2003 9:00 pm
Location: Bay City, Michigan
Contact:

Postby Pat Loboda » Fri Oct 24, 2003 12:34 pm

Bobbie,

Are you spraying your bottles with SuperSpray or SprayA before slumping?

Thanks,
Pat Loboda

charlie
Posts: 961
Joined: Mon Mar 10, 2003 3:08 pm

Postby charlie » Fri Oct 24, 2003 12:37 pm

Pat Loboda wrote:Bobbie,

Are you spraying your bottles with SuperSpray or SprayA before slumping?

Thanks,
Pat Loboda


i spray only the top side with borax to prevent devit

BobbieMatus
Posts: 50
Joined: Tue Jul 08, 2003 12:21 am

spraying bottles

Postby BobbieMatus » Fri Oct 24, 2003 3:16 pm

I don't spray my bottles. I have slumped about 70 and have never had devit.
Bobbie

Joanne Owsley
Posts: 52
Joined: Wed Apr 16, 2003 4:27 pm
Location: Arlington, WA
Contact:

Postby Joanne Owsley » Fri Oct 24, 2003 9:26 pm

I use a schedule similar to the one you posted, but I anneal at 1050. This sched gives me few, if any bubbles. I've tried going faster from 1100 to fusing, but it only gave me more bubbles. :roll:
~ Joanne

"What neglected medication made you think THAT was a good idea??"
- me, to myself

BobbieMatus
Posts: 50
Joined: Tue Jul 08, 2003 12:21 am

Postby BobbieMatus » Fri Oct 24, 2003 9:31 pm

I tried the new schedule and I'm not getting bubbles, maybe because I fire on thin fire. Have you tried holding longer at 1100? Ramping full power from 1100 up cut 1 hour off the total time.
Bobbie :lol:

Susan Slack
Posts: 13
Joined: Wed Apr 02, 2003 10:10 am
Location: Green Oaks, Il.

Postby Susan Slack » Fri Oct 24, 2003 9:39 pm

I just throw them in with my regular fuse firings when I have an empty spot in the kiln. Never have any problem. Clear ones are blah. Sometimes a little divit. Mostly ok. Susan
Susan from Green Oaks

BobbieMatus
Posts: 50
Joined: Tue Jul 08, 2003 12:21 am

Postby BobbieMatus » Fri Oct 24, 2003 9:56 pm

I do the bottles separate, can fit 5 to 6 at a time depending on size of the bottle. Clear ones are blah, and they don't sell, neither do the amber. People seem to like the green and the blue the best.
Bobbie

Joanne Owsley
Posts: 52
Joined: Wed Apr 16, 2003 4:27 pm
Location: Arlington, WA
Contact:

Postby Joanne Owsley » Fri Oct 24, 2003 10:22 pm

[quote="luvhug"]I tried the new schedule and I'm not getting bubbles, maybe because I fire on thin fire. Have you tried holding longer at 1100? Ramping full power from 1100 up cut 1 hour off the total time.
Bobbie :lol:[/quote]

The bubbles to which I was referring are bubbles inside the bottle, from air getting trapped inside. The only way I've been able to avoid them is to go slow from 1100 to fusing temp. I'm open to any suggestions, though.
~ Joanne



"What neglected medication made you think THAT was a good idea??"

- me, to myself

BobbieMatus
Posts: 50
Joined: Tue Jul 08, 2003 12:21 am

Postby BobbieMatus » Fri Oct 24, 2003 10:33 pm

Hmmm, that's the bubble squeeze going slow from 1100 to fusing temp. The only thing I can suggest is maybe holding longer at the 1100, 20 or 30 min. I thought I would have that problem too when I switched, but I didn't. There has to be other people out there doing bottles. What's everyone using for their firing schedule?
Bobbie


Post Reply

Return to “Techniques and Tools”

Who is online

Users browsing this forum: No registered users and 51 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com