Hello all,

I would like to fuse (sandwich) thin copper wire between 2 sheets of 3mm glass and then slump into a shallow platter shape.

This would be 2 firings.

Will then wire inside the glass slump together with the glass? Or will the glass and wire separate out during the slump?

Pete
Peter Angel
http://peterangelart.blogspot.com/

A bigger kiln, A bigger kiln, my kingdom for a bigger kiln.

charlie
Posts: 961
Joined: Mon Mar 10, 2003 3:08 pm

Re: Fusing wire between 2 sheets and then slumping

Postby charlie » Wed Jun 10, 2015 10:47 pm

it will slump but not stretch. if the drop is too much and causes the glass to stretch, then the wires can be pulled to the surface or even out of the glass. the wires will act like a wire melt in that case.

Judith Andre
Posts: 28
Joined: Thu Mar 20, 2003 2:38 am
Location: Lincoln, NE

Re: Fusing wire between 2 sheets and then slumping

Postby Judith Andre » Fri Jun 19, 2015 1:46 am

In my experience, the glass will break because it moves, the wire does not.
Judith


Post Reply

Return to “Techniques and Tools”

Who is online

Users browsing this forum: No registered users and 55 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com