Postby Drewcilla » Sun Jul 05, 2015 7:25 pm

I put a 3mm Bullseye screen-printed 3 1/2 in square piece in my Paragon Caldera to fire. Went full to 1050 with a 10 minute hold. Then my schedule is full to 1465. However, at about 1100 I looked through the peephole to see how the enamel was looking and saw black specks all over the piece and shelf paper. I immediately turned it off completely figuring the piece was ruined. My experience is that kiln crap gets embedded into the glass.

When I took the piece out I found that the specks brushed off nicely. I'm wondering if I can refire the piece or is the integrity of the piece compromised because i did not do a regular anneal?

Thanks so much.
Drewcilla

Brad Walker
Site Admin
Posts: 1348
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: Firing aborted; can I refire

Postby Brad Walker » Mon Jul 06, 2015 8:14 am

No problem with refiring.

Also, a 3mm piece of glass will anneal just fine cooling gradually through the annealing range.

Drewcilla
Posts: 60
Joined: Fri Apr 11, 2008 9:10 am

Re: Firing aborted; can I refire

Postby Drewcilla » Mon Jul 06, 2015 10:57 am

Thanks Brad.

Warren Weiss
Posts: 137
Joined: Thu Mar 13, 2003 8:06 pm
Location: Richmond, VA

Re: Firing aborted; can I refire

Postby Warren Weiss » Mon Jul 06, 2015 12:58 pm

Better find out what the black specks are and eliminate them. While they won't embed in the glass at 1100, they will at 1465.

Warren

Rick Wilton
Posts: 273
Joined: Sat Oct 25, 2003 8:18 pm
Location: Calgary, Canada
Contact:

Re: Firing aborted; can I refire

Postby Rick Wilton » Mon Jul 06, 2015 2:03 pm

I'd think that the black specs were ash that came from the SHELF PAPER. This likely happens every time you use shelf paper but completely burns out by the time you see the finished results.
Rick Wilton

Warren Weiss
Posts: 137
Joined: Thu Mar 13, 2003 8:06 pm
Location: Richmond, VA

Re: Firing aborted; can I refire

Postby Warren Weiss » Mon Jul 06, 2015 4:47 pm

I know that thinfire turns black around 800 f and goes back to white at higher temperatures. I never noticed it deposit on the glass.

Warren

Bert Weiss
Posts: 2337
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: Firing aborted; can I refire

Postby Bert Weiss » Mon Jul 06, 2015 6:47 pm

Warren Weiss wrote:Better find out what the black specks are and eliminate them. While they won't embed in the glass at 1100, they will at 1465.

Warren

By 1465, they have burned up. Carbon with heat and oxygen, vaporizes. I have seen it stick in a situation where there is no oxygen, only heat. (that would be under very large sheets of glass) But the general rule is no sticking.
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions

Warren Weiss
Posts: 137
Joined: Thu Mar 13, 2003 8:06 pm
Location: Richmond, VA

Re: Firing aborted; can I refire

Postby Warren Weiss » Mon Jul 06, 2015 7:15 pm

Bert,

If pure carbon, you are surely correct. If it is black rust it is another story. Just saying that I have never seen carbon from thin fire deposit on the glass, but I suppose it could.

Warren

Bert Weiss
Posts: 2337
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: Firing aborted; can I refire

Postby Bert Weiss » Mon Jul 06, 2015 10:21 pm

Warren Weiss wrote:Bert,

If pure carbon, you are surely correct. If it is black rust it is another story. Just saying that I have never seen carbon from thin fire deposit on the glass, but I suppose it could.

Warren

I have seen carbon from Unifrax 970 paper make permanent marks on glass. It was on large sheets. I prefire when making complex patterns on large sheets, using fiber papers.
Bert



Bert Weiss Art Glass*

http://www.customartglass.com

Furniture Lighting Sculpture Tableware

Architectural Commissions


Post Reply

Return to “Techniques and Tools”

Who is online

Users browsing this forum: No registered users and 36 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com