How to polish a tiny spot

Postby Don Burt » Sat Dec 03, 2016 1:03 pm

I get an occasional spot of crap on my otherwise clear glass. If I remove the crap with a little diamond bit, e.g. a 220 grit burr from HIS Glassworks, I now have a little white spot. Is there a way to polish this little speck so that I will have a little polished divot instead of a white dot?

DonMcClennen
Posts: 369
Joined: Sun Mar 09, 2003 9:09 pm
Location: Ontario

Re: How to polish a tiny spot

Postby DonMcClennen » Sat Dec 03, 2016 1:21 pm

Try a little spot of clear nail polish
"The Glassman"

Kevin Midgley
Posts: 713
Joined: Mon Mar 10, 2003 11:36 am
Location: Tofino, British Columbia, Canada

Re: How to polish a tiny spot

Postby Kevin Midgley » Sat Dec 03, 2016 4:13 pm

use a razor blade.
won't leave a divot.
If the blade doesn't remove it so you cannot feel it, you have a problem!
If you worry about scratching, round off the corners of the blade first so it won't scratch.

peter cummings
Posts: 67
Joined: Mon Jan 19, 2004 4:05 am
Location: sale,s.e.vic,australia
Contact:

Re: How to polish a tiny spot

Postby peter cummings » Sun Jan 01, 2017 1:18 am

If you have a tiny whitish spot after using a 220 grit burr. I found those rubberised polishing burrs messy, and hard to keep to a small spot. If you have a drill with a collet chuck, I love my foredom, you can use small wood or bamboo pieces in it with loose grit. 400 or finer then pumice or cerium. Matches or I get thin bamboo from sushi mats. Reason I prefer the collet is if it breaks it's easy to get the broken bit out. A bit of water, gently. If your drill has bigger collets, Foredom again, You can use 1/4 inch dowel shaped to a round end or a point. Very precise. (engravers can get anal over detail)

Buttercup
Posts: 561
Joined: Mon Jan 28, 2008 5:22 pm
Location: S.E. Queensland Australia

Re: How to polish a tiny spot

Postby Buttercup » Sat Feb 11, 2017 10:33 pm

Don, could you paint something (a fig leaf?) over the offending spot and then refire?

Your artwork is usually very organic so modifying the design slightly might be a lot less arduous than trying to get back to shiny clear glass.

Jen

Ed Cantarella
Posts: 155
Joined: Mon Feb 26, 2018 3:49 pm
Location: Highland, Michigan, USA

Re: How to polish a tiny spot

Postby Ed Cantarella » Wed Apr 18, 2018 2:33 pm

220 seems fairly aggressive (to me :) ). 800 grit burrs are easy to find. Diamond powder with a little carrier(oil) using the wood stick in drill(dremel) chuck is good for small round spots. https://lascodiamond.com/LascoProducts- ... owder.html A gram of diamond dust is about 1/2 a thimble full. Enough for a lot of spots.
*Many stores(especially those $1 stores) carry bamboo toothpicks - much strong than wood.
HER last words were, "I'm melting, melting . . . " Dissenting opinions generally welcome for comic relief or personal edification. Sometimes both.


Post Reply

Return to “Techniques and Tools”

Who is online

Users browsing this forum: Google [Bot] and 68 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com

cron