I am fusing two large sheets of Bullseye White (013-30) together. They are 13" x 29". Do I need to adjust the fusing schedule due to the size?
Dick
Posts: 89
Joined: Sun May 01, 2005 9:34 pm
Location: San Diego
Contact:

Re: fusing large sheets

Post by Dick »

unless there is texture or something else that you need a bubble squeeze on no. otherwise fairly slow to 1200, soak an hour and go. Also depends on if you are close to the elements