For some works where I have considered the back side critical, I have"casted"
the kiln wash.
I take a sheet of float glass, clean it and apply car wax which I polish carefully.
Then I cast a layer of gypsum. It will get an almost glossy surface. There gypsum plates i use for carving a pattern I want ti "print" on glass.
For minor works like cabochons, I also use a float glass as amould. I paint it with thick kilnwash, with a rolling pin press a 2-3 mm fiber paper into the wet kilnwash. Then i let it dry and peel the fiber paper carefully off. It leaves a nice
surface although it odten sticks into piece. Soaking overnight in a dilute phosphoric acid like Cocacola softens the contamination and it is easy to wash off.
-lauri
the kiln wash.
I take a sheet of float glass, clean it and apply car wax which I polish carefully.
Then I cast a layer of gypsum. It will get an almost glossy surface. There gypsum plates i use for carving a pattern I want ti "print" on glass.
For minor works like cabochons, I also use a float glass as amould. I paint it with thick kilnwash, with a rolling pin press a 2-3 mm fiber paper into the wet kilnwash. Then i let it dry and peel the fiber paper carefully off. It leaves a nice
surface although it odten sticks into piece. Soaking overnight in a dilute phosphoric acid like Cocacola softens the contamination and it is easy to wash off.
-lauri
Re: Sticky cabochons: shelf paper vs kiln wash again
Fascinating, Lauri. Although I must admit that the first thing I thought was, "And we DRINK Cocacola?"

Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
-
Lauri Levanto
- Posts: 270
- Joined: Tue Mar 11, 2003 7:33 am
- Location: Halikko, Finland
Re: Sticky cabochons: shelf paper vs kiln wash again
So do I, too.Morganica wrote:"And we DRINK Cocacola?"
And I even smoke tobacco.
There are plenty of dangerous stuff we consume, chili for example.
They kill slowly, but I am retired, no need to hurry.
Ps.
The decalcinating stuff used for kitchenware is much cheaper.
-
jim simmons
- Posts: 478
- Joined: Sun Mar 09, 2003 10:37 pm
- Location: Hillsboro Oregon
- Contact:
Re: Sticky cabochons: shelf paper vs kiln wash again
Also white vinegar works just fine
Jim
Jim
Lauri Levanto wrote:For some works where I have considered the back side critical, I have"casted"
the kiln wash.
I take a sheet of float glass, clean it and apply car wax which I polish carefully.
Then I cast a layer of gypsum. It will get an almost glossy surface. There gypsum plates i use for carving a pattern I want ti "print" on glass.
For minor works like cabochons, I also use a float glass as amould. I paint it with thick kilnwash, with a rolling pin press a 2-3 mm fiber paper into the wet kilnwash. Then i let it dry and peel the fiber paper carefully off. It leaves a nice
surface although it odten sticks into piece. Soaking overnight in a dilute phosphoric acid like Cocacola softens the contamination and it is easy to wash off.
-lauri