Super Spray Streaking

Postby tgotch » Mon Jan 27, 2014 11:29 am

I have been testing Super Spray A for my bottle devit issues (I usually use Borax concoction with fair success).

I brush on Super Spray with a foam brush, then fire to 1430. The gloss looks good, but the bottles have brush streaks in the glass after firing.

Anyone have suggestions to eliminate the streaks?

vblue
Posts: 98
Joined: Sun Mar 09, 2003 11:05 pm
Location: Texas

Re: Super Spray Streaking

Postby vblue » Mon Jan 27, 2014 4:51 pm

Go to Michael's or a craft store or art store and get a Badger air brush kit. Makes it a lot easier to use and no streaks. Helps to have a 40% off coupon for Michael s too.

Laurie Spray
Posts: 321
Joined: Sat Dec 17, 2005 10:32 pm
Location: SANTA CRUZ, CALIFORNIA
Contact:

Re: Super Spray Streaking

Postby Laurie Spray » Wed Jan 29, 2014 12:52 am

Spray for sure!
Laurie Spray

New website!! Http://bonnydoonfusedglasstools.com
Maker of stainless steel rings,pattern bar formers, pot melt pots, and Bottomless Molds
glass: http://lauriespray.blogspot.com

tgotch
Posts: 36
Joined: Mon Nov 14, 2011 11:04 pm

Re: Super Spray Streaking

Postby tgotch » Wed Jan 29, 2014 10:36 pm

Thanks for the tip. I bought a Badger 250-2 with a compressed air can to try (whole setup cost me ~$30 with coupon from Michaels.).
Results were much better.
I Just need a bit more practice to get more proficient with using the airbrush.

Valerie Adams
Posts: 587
Joined: Mon Apr 19, 2004 2:49 pm
Location: Santa Rosa, California
Contact:

Re: Super Spray Streaking

Postby Valerie Adams » Thu Jan 30, 2014 1:00 am

And make sure you're shaking the container frequently. Using a brush means you're probably picking up more of the glass in the bottom of your container.


Post Reply

Return to “Newcomer Forum”

Who is online

Users browsing this forum: No registered users and 12 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com