Does this fusing mold need air holes?

Postby Shelley Lewis » Wed Feb 12, 2014 8:27 pm

I plan to full fuse on the kiln shelf first, then slump into this spiral mold. The website that sells it states that fusing can be done directly on the mold, but I'm a little apprehensive about trying it the first time. Should I drill holes, and how many?
Thanks for all the great advice!
Attachments
image.jpg

lorimendenhall
Posts: 91
Joined: Wed Apr 10, 2013 8:54 pm
Location: Orange County, CA
Contact:

Re: Does this fusing mold need air holes?

Postby lorimendenhall » Wed Feb 12, 2014 9:58 pm

I doubt it needs holes. I full fuse onto a texture plate and there are no holes and it's fine. Also, I've got plenty of shallow slump molds that don't have holes.

jvbs
Posts: 8
Joined: Sat Jan 11, 2014 12:36 pm

Re: Does this fusing mold need air holes?

Postby jvbs » Sun Mar 09, 2014 12:40 pm

I would love to know where to get this mold!

Shelley Lewis
Posts: 73
Joined: Wed Dec 11, 2013 11:14 am

Re: Does this fusing mold need air holes?

Postby Shelley Lewis » Sun Mar 09, 2014 1:42 pm

jvbs wrote:I would love to know where to get this mold!


Delphiglass.com

beninfl
Posts: 46
Joined: Sat Feb 08, 2014 8:54 pm

Re: Does this fusing mold need air holes?

Postby beninfl » Sun Mar 09, 2014 5:36 pm


linn keller
Posts: 52
Joined: Mon Mar 10, 2003 12:22 pm
Location: south tx

Re: Does this fusing mold need air holes?

Postby linn keller » Sun Mar 09, 2014 10:42 pm

I seem to recall that not so long ago, maybe a couple of months? , the someone posted here with a pic of this mold and glass with bubbles. The person had followed the instructions but it still bubbled up. The general consensus was that even though the instructions say no problem to fuse/slump all in one, it would probably be far better to do two separate processes. Good luck,
Linn
linn in deep deep south texas

Glass Fever
Posts: 29
Joined: Sat Aug 04, 2007 11:08 pm
Location: Chicago Suburbs
Contact:

Re: Does this fusing mold need air holes?

Postby Glass Fever » Sun Mar 09, 2014 10:52 pm

linn keller wrote:I seem to recall that not so long ago, maybe a couple of months? , the someone posted here with a pic of this mold and glass with bubbles. The person had followed the instructions but it still bubbled up. The general consensus was that even though the instructions say no problem to fuse/slump all in one, it would probably be far better to do two separate processes. Good luck,
Linn


Yes, that was the OP, that thread was posted a few days after this one. :)

jvbs
Posts: 8
Joined: Sat Jan 11, 2014 12:36 pm

Re: Does this fusing mold need air holes?

Postby jvbs » Mon Mar 10, 2014 9:45 am

I remember this mold now. I didn't pay much attention because I have a very small kiln and this mold is too large. Does anyone know of a labyrinth type mold 6" or smaller?

JestersBaubles
Posts: 696
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: Does this fusing mold need air holes?

Postby JestersBaubles » Thu May 29, 2014 10:59 pm

Gil Reynolds has made a video that gives some tips/techniques for using this mold:

http://youtu.be/7Am6s6wl7jI

Dana W.

Laurie Spray
Posts: 321
Joined: Sat Dec 17, 2005 10:32 pm
Location: SANTA CRUZ, CALIFORNIA
Contact:

Re: Does this fusing mold need air holes?

Postby Laurie Spray » Sun Jun 01, 2014 8:54 pm

We can make it for you. Email me
Laurie Spray

New website!! Http://bonnydoonfusedglasstools.com
Maker of stainless steel rings,pattern bar formers, pot melt pots, and Bottomless Molds
glass: http://lauriespray.blogspot.com


Post Reply

Return to “Newcomer Forum”

Who is online

Users browsing this forum: No registered users and 8 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com