Postby Chris Lowry » Tue Oct 03, 2017 5:14 pm

Sorry for the stupid question but I can't really find what I'm looking for with the search function.

What type of plaster do you use to cast with? I know there are products from R&R but I'm just wondering about plaster silica type molds.

What I understand is dental plaster is good but I also read somewhere that Hydrostone plaster is the same. Is that true?

I've also heard that casting plaster is good... is that the same as 20 minute casting plaster?

Thanks for any help that might be out there.

JestersBaubles
Posts: 642
Joined: Fri Feb 25, 2011 12:01 am
Location: North Logan, UT
Contact:

Re: plaster for casting

Postby JestersBaubles » Fri Oct 13, 2017 10:39 pm

50/50 mixture of pottery plaster and silica. Both can be purchased cheaply from any pottery supply.

Dana W.

Chris Lowry
Posts: 49
Joined: Thu Sep 24, 2015 12:35 pm

Re: plaster for casting

Postby Chris Lowry » Sat Oct 14, 2017 12:08 am

Thanks... that's what I ordered but it will be awhile before I get to try it.

heywilli
Posts: 3
Joined: Tue Jul 16, 2013 9:10 pm

Re: plaster for casting

Postby heywilli » Tue Nov 28, 2017 8:38 pm

Hi I typically use Hydrocal and silica flour 1:1 for the first layer if hand building and then add an equal amount of silica sand to the silica flour or hydrocal. I find that this makes pretty strong molds that divest quiet easily. If I am making a larger mold and I worry about mold cracking, for hand built molds I will first make several layers of plaster and then dip drywall tape pieces into the wet plaster mix and apply this around the mold and then cover with another layer of plaster for a total of about 4 layers of plaster. If you cannot find Hydrocal then pottery plaster works fine as well. This is much more economical that using the R & R mix and I find I get clean castings with this mixture which are easily divested. Hope this helps.

Don Burt
Posts: 487
Joined: Sun Mar 09, 2003 8:45 pm
Location: Cincinnati, Ohio
Contact:

Re: plaster for casting

Postby Don Burt » Wed Nov 29, 2017 1:08 pm

heywilli wrote:Hi I typically use Hydrocal and silica flour 1:1 for the first layer if hand building and then add an equal amount of silica sand to the silica flour or hydrocal. I find that this makes pretty strong molds that divest quiet easily. If I am making a larger mold and I worry about mold cracking, for hand built molds I will first make several layers of plaster and then dip drywall tape pieces into the wet plaster mix and apply this around the mold and then cover with another layer of plaster for a total of about 4 layers of plaster. If you cannot find Hydrocal then pottery plaster works fine as well. This is much more economical that using the R & R mix and I find I get clean castings with this mixture which are easily divested. Hope this helps.


You put plaster molds with drywall tape in them into a kiln? Nothing bad happens? Smoke issues?

Peter Angel
Posts: 186
Joined: Fri Oct 31, 2008 9:26 am
Location: Newtown, Sydney, Australia.

Re: plaster for casting

Postby Peter Angel » Thu Nov 30, 2017 2:25 am

Make sure you get pottery plaster Number 1.

Its much stronger than regular plaster
Peter Angel
http://peterangelart.blogspot.com/

A bigger kiln, A bigger kiln, my kingdom for a bigger kiln.


Post Reply

Return to “Kiln Casting”

Who is online

Users browsing this forum: No registered users and 4 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com