Hi, we lived abroad for 7 years and I am just now returning to glasswork. My equipment and supplies were in a storage facility without heat or a/c. I fired my first pieces and they all migrated to the middle of the kiln shelf and fused together. I used the Basic 6 schedule from this site BASIC 6-Segment Firing Schedules.
http://system96.com/Resources/FiringGuideFahrenheit.pdf with System 96 glass. I suspect the temp was too high but fear there might be other contributing factors.
I used Thinfire shelf paper that no longer looks white from being in storage so long. It looks beige. Does shelf paper deteriorate?
I used to fire my kilns in my kitchen but have room in the garage in our new house. It was colder (low of 40 F0 and rainy when I fired. Does the garage need to be heated?
Thanks in advance for your kind assistance.
Diane
Troubleshooting
Moderator: Brad Walker
Troubleshooting
- Attachments
-
- FullSizeRender.jpg (31.33 KiB) Viewed 16909 times
-
DonMcClennen
- Posts: 381
- Joined: Sun Mar 09, 2003 9:09 pm
- Location: Ontario
Re: Troubleshooting
It should not make any difference what's going on outside (rain, cold etc.) It's what's going on inside the kiln that counts! If all pieces migrated toward centre then I suggest you have some kind of vibration going on. Put just a few pieces back in and run a monitored test firing.. try to figure out what is causing garage floor/kiln vibration. Check to make sure your kiln shelf is level. Storing a kiln should not cause any problems... yours looks to be in good shape!
"The Glassman"
Re: Troubleshooting
Thinfire shrinkage is my guess.
(oops, Jim Hobbyist got it first)
(oops, Jim Hobbyist got it first)
Re: Troubleshooting
Thank you both for your input. I will try another fire with scrappy pieces and keep you posted.