Sticking stacked glass.
I slump float glass over stainless steel molds. Hi-Temp 1800 works great on the mold. When I slump 2 pieces of glass stacked, I spray a light coat of  Hi Temp 1800 on one of them but it  leaves a haze that is difficult to remove. Any suggestions to keep the glass from sticking to each other ?  Thanks Mike
			
			
									
						
										
						- 
				JestersBaubles
- Posts: 705
- Joined: Fri Feb 25, 2011 12:01 am
- Location: North Logan, UT
- Contact:
Re: Sticking stacked glass.
Why would you stack two pieces of glass on top of each other, and not want them to fused together? 
The boron nitride spray is for coating molds, not glass. I suppose you could use 1/8" fiber paper between the two pieces if you are really bent on fusing two at a time.
From my experience, Hi Temp 1800 is inferior to MR-97. Every time I've used the High Temp it has clouded my glass like you suggest. MR-97 does not do that (in my experience).
Dana W.
			
			
									
						
										
						The boron nitride spray is for coating molds, not glass. I suppose you could use 1/8" fiber paper between the two pieces if you are really bent on fusing two at a time.
From my experience, Hi Temp 1800 is inferior to MR-97. Every time I've used the High Temp it has clouded my glass like you suggest. MR-97 does not do that (in my experience).
Dana W.
- 
				Mike Bathalter
- Posts: 2
- Joined: Mon Feb 03, 2014 5:31 pm
Re: Sticking stacked glass.
Thanks Dana, I stack the glass so it doubles the amount pieces made in each firing. 
I have used Thin Fire paper but that gets expensive.
I am not familiar with MR- 97 but will give a try . Thanks again ! Mike
			
			
									
						
										
						I have used Thin Fire paper but that gets expensive.
I am not familiar with MR- 97 but will give a try . Thanks again ! Mike
Re: Sticking stacked glass.
Try sifting down a separator--dry kilnwash, plaster of paris, alumina, that sort of thing. If you coat it well (and evenly) you should get separation without the expense of BN.
			
			
									
						
							Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
			
						Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
- 
				Lauri Levanto
- Posts: 270
- Joined: Tue Mar 11, 2003 7:33 am
- Location: Halikko, Finland
Re: Sticking stacked glass.
That is how windshields are made.Morganica wrote:Try sifting down a separator--dry kilnwash, plaster of paris, alumina, that sort of thing. If you coat it well (and evenly) you should get separation without the expense of BN.
- 
				rosanna gusler
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
Re: Sticking stacked glass.
you can also make a wash with pure alumina and a binder (cmc, elmers glue, sugar) for green strength and spray on a smooth coat. let dry and stack. r.
			
			
									
						
							artist, owner of wanchese art studio, marine finisher