pieced dish splits during slumping fire

Postby conboc » Fri Nov 13, 2015 4:06 pm

The fusing firing looked ok. During he slump firing the dish split apart pretty much along the seam of the top glass. I used two 3mm layers of COE 90 glass.
The slump firing schedule was:
250 to 350 soak for 12 min
350 to 750 soak for 22 min
FULL to 1400 soak for 15 min
FULL to 900 soak for 1 hr.
100 to 70 soak 1 min.
Attachments
broken-dish.jpg

Marty
Posts: 855
Joined: Mon Mar 10, 2003 3:58 pm
Location: Maine
Contact:

Re: pieced dish splits during slumping fire

Postby Marty » Fri Nov 13, 2015 5:02 pm

Too fast. Too hot.
Please tell us where you got that schedule.

David Jenkins
Posts: 174
Joined: Wed Apr 29, 2009 10:35 pm
Location: Cypress, Texas

Re: pieced dish splits during slumping fire

Postby David Jenkins » Fri Nov 13, 2015 7:25 pm

What do you mean by "seam" of the top glass - was it two pieces that you fused together? Also: In the picture, it looks like the bottom was of two colors - is that correct? Or is the black-looking right hand side just an artifact of the camera shot?
Dave Jenkins
Glass at Harbor Gates
Cypress, TX

conboc
Posts: 11
Joined: Wed Apr 08, 2015 12:17 am

Re: pieced dish splits during slumping fire

Postby conboc » Sat Nov 14, 2015 8:45 am

Marty,

I can’t find where I got that schedule now. I either took it off the metallic decal instructions, or I made a huge mistake when I copied whatever schedule I was looking at. It certainly isn’t the bullseye one for slumping. I do have to fire a bit hot in my small kiln to get full fuses, I had one decal flake off, so I bumped up the heat a bit for the high fire metallic decal.

David,

Yes, it is 4 pieces of glass: two on top, two on the bottom and the seam for both layers was in the same place. Was that stupid maybe?

I really, really appreciate you fellows help, as I there is no place near me to take classes.

David Jenkins
Posts: 174
Joined: Wed Apr 29, 2009 10:35 pm
Location: Cypress, Texas

Re: pieced dish splits during slumping fire

Postby David Jenkins » Sat Nov 14, 2015 11:51 am

I would think that the markedly different colors would require an especially slow schedule, since the two colors absorb heat at significantly different rates. That would cause undue stress to occur at the joint line.
Dave Jenkins
Glass at Harbor Gates
Cypress, TX

Jerrwel
Posts: 129
Joined: Thu Feb 10, 2005 6:25 pm
Location: Charlotte, NC

Re: pieced dish splits during slumping fire

Postby Jerrwel » Sat Nov 14, 2015 2:10 pm

conboc wrote:as there is no place near me to take classes.


Classes are not a panacea; they are typically fun and some good information is available. Growing to understand the interplay of design, glass and firing processes is essential. Several books present keys to successful glass fusing well. Brad's 'Contemporary Fused Glass' http://www.warmglass.org/books goes through steps actively providing understanding of various fusing process basics; the Wardells' book, 'Joy of Fusing' focuses on some easy projects using different processes and not requiring a full fuse on all of the projects. Both books look at the understanding and development of firing schedules so that one does not need to blindly trust a schedule provided. The eventual advanced step is to read, read, read, and use 'Firing Schedules for Glass' by Graham Stone; a single read is not sufficient and understanding the variables within glass and glass projects (such as glass elements within a project absorbing heat at differing rates) presented in this book is essential to becoming independent in designing and executing fusing projects. While information regarding a particular glass or design element is needed, Stone's book helps one integrate that information with knowledge of other project variables to determine what is likely to be a successful firing schedule.

There are several axioms that are true to fusing; here are two, (1) 'low and slow,' and (2) 'more is learned from failure than success.' 'Hurry up and wait' schedules containing numerous holds during firing stages are contrary to the 'low and slow' mantra and I avoid them. Painfully accept that failure is part of learning and learning never stops.
Jerry

conboc
Posts: 11
Joined: Wed Apr 08, 2015 12:17 am

Re: pieced dish splits during slumping fire

Postby conboc » Sat Nov 14, 2015 8:38 pm

thank you for your help.
Appreciate the book recommendations.

Valerie Adams
Posts: 587
Joined: Mon Apr 19, 2004 2:49 pm
Location: Santa Rosa, California
Contact:

Re: pieced dish splits during slumping fire

Postby Valerie Adams » Sun Nov 15, 2015 7:48 pm

conboc wrote:Yes, it is 4 pieces of glass: two on top, two on the bottom and the seam for both layers was in the same place. Was that stupid maybe?


I wouldn't go so far as to use the word stupid, but there's no need for the top layer to be two pieces, especially since you're placing a decal on top. The top layer could've just been a single piece of clear which would also help to hold the two bottom pieces together, assuming a successful first firing.

conboc
Posts: 11
Joined: Wed Apr 08, 2015 12:17 am

Re: pieced dish splits during slumping fire

Postby conboc » Sun Nov 22, 2015 8:22 pm

thanks Val,
I've made two more dishes and used a solid piece of clear for the top, and yes, that is working fine. I am realizing that design choices need to be tempered with practicality, at least for a beginner.

And I am SO thankful for the earlier suggestion to get Brad Walkers book! It is WONDERFUL. It contains so much useful information all in one place. its clear, concise an deasy to understand. Even things I already know something about are so much more clear now. What a wonderful find. I can't put it down.


Post Reply

Return to “Newcomer Forum”

Who is online

Users browsing this forum: No registered users and 10 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com