Here I am again.
Just fused a plate, and on some parts of the cut pieces, there's a white outline. Is this devit? The base is clear with transparent pieces added.
Thanks again.
Kay
white outline
Moderators: Brad Walker, Tony Smith
-
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
If the edges are ground, it is snall glass particles which always read white. Grind to a finer grit before fiiring.Els VandenEnde wrote:Hi Kay,
It's quite possibly devit, especially if you ground the edges or cut the pieces out with a ring saw.
Els
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
- Posts: 340
- Joined: Mon Mar 10, 2003 4:16 pm
- Location: Northern CA
- Contact:
White outline
Thanks again- I'll do all of the above. Kay
-
- Posts: 195
- Joined: Mon Mar 10, 2003 9:45 pm
- Location: SW FL
- Contact:
white outline
Thanks Judy! Super Spray on order.