Re: Alternate Frit Maker - any downsides?
Posted: Mon Jan 21, 2013 5:07 pm
Garbage disposals work great. I have run hundreds of pounds through mine - Kitchenaid rescued from the trash. The secret is using lots of water - I simply connected a hose fitting on the dishwasher drain pipe port. I run the resulting ground glass through a screen with water to separate out the fines. I do this in my shop sink which I installed a plaster trap on. I then dry the frit on large metal trays. Air drying works best but is slow - sometimes I will place the trays in a conventional oven at around 250 degrees. I then run the dried frit through 3 different lab test sieves - 2mm, 1mm, and .5mm with a bottom pan and lid. Thinner glass processes better through the disposal in general. Tramp iron is a big concern and is easily removed with a high quality rare earth magnet.