Why would devitrification develop there? Is there more stress in those areas already? I wonder if I should not use this batch of gold purple I have, the side with the pattern will have to be the top of the piece to have smooth sides together. Hmmm, but it appeared on other colors as well. Just more ...
- Wed Oct 01, 2003 8:41 pm
- Forum: Techniques and Tools
- Topic: cool devit...and how to get rid of it
- Replies: 13
- Views: 11297
Mystery solved...mostly
I have been racking my brain as to what contaminated my shelf or glass to get this crazy devit pattern, and then this evening in the studio I picked up a fresh piece of BE gold purple and lo and behold....THE PATTERN! http://www.glasskitchen.com/auction/lissa/purple.jpg http://www.glasskitchen.com/a...
- Wed Oct 01, 2003 12:42 pm
- Forum: Techniques and Tools
- Topic: cool devit...and how to get rid of it
- Replies: 13
- Views: 11297
- Wed Oct 01, 2003 12:39 pm
- Forum: Techniques and Tools
- Topic: cool devit...and how to get rid of it
- Replies: 13
- Views: 11297
- Wed Oct 01, 2003 11:43 am
- Forum: Techniques and Tools
- Topic: cool devit...and how to get rid of it
- Replies: 13
- Views: 11297
cool devit...and how to get rid of it
I have a 13" disc 1/4" thick that developed devitrification in a an attempt to fire polish. I brought the piece to full fuse, no problem, and then flipped it and set a fire polish cycle as I wanted the 'top' to become the 'bottom'. Devitrification developed on BE transparent orange and bla...
- Fri Sep 26, 2003 7:51 am
- Forum: Techniques and Tools
- Topic: Kiln wash: ceramic vs glass
- Replies: 8
- Views: 9783
- Mon Sep 15, 2003 12:18 pm
- Forum: Techniques and Tools
- Topic: Super Spray
- Replies: 7
- Views: 7995
- Mon Sep 15, 2003 11:29 am
- Forum: Techniques and Tools
- Topic: Super Spray
- Replies: 7
- Views: 7995
- Mon Sep 15, 2003 7:52 am
- Forum: Techniques and Tools
- Topic: Silkscreening on Glass
- Replies: 12
- Views: 13652
- Thu Sep 11, 2003 12:43 pm
- Forum: Techniques and Tools
- Topic: Help please! My first Devit experience....i think....
- Replies: 11
- Views: 8773
- Fri Sep 05, 2003 6:58 pm
- Forum: Techniques and Tools
- Topic: BE shelf/mold wash
- Replies: 2
- Views: 2939
- Fri Sep 05, 2003 4:59 pm
- Forum: Techniques and Tools
- Topic: BE shelf/mold wash
- Replies: 2
- Views: 2939
BE shelf/mold wash
I am using BE wash for the first time and have a few questions. 1) I used the ratio of powder to water they suggest (4 to 1) and read the instructions to put on four coats for a previously fired item....four coats of that ratio wash BARELY gave the shelf a pink tint. I added lots more powder and put...
- Thu Sep 04, 2003 6:17 pm
- Forum: Techniques and Tools
- Topic: insulation for studio wall question
- Replies: 22
- Views: 20417
Wow, I did a slump fire this afternoon and my kiln dropped from 1300 to 1050 in under half hour an hour. Hope I didn't overslump, but even if so I can just work that into a new equation. I'll have to see how a fuse fire goes tomorrow. The clothes on the drying rack are going to take longer to dry no...
- Thu Sep 04, 2003 12:03 pm
- Forum: Techniques and Tools
- Topic: insulation for studio wall question
- Replies: 22
- Views: 20417
- Thu Sep 04, 2003 11:30 am
- Forum: Techniques and Tools
- Topic: insulation for studio wall question
- Replies: 22
- Views: 20417
I am very interested to hear more on the topic of NOT flash venting, I understood it to be pretty important to avoid devit. My kiln is my laundry room and I would love to skip the flash venting. It's not too fun either! I guess too, a matter of time, my kiln loses heat pretty slowly and I imagine no...
- Mon Sep 01, 2003 8:25 pm
- Forum: Techniques and Tools
- Topic: Moretti - New Colours
- Replies: 4
- Views: 4992
Here's a link that should help you out
http://www.cauldroncreations.com/pasteleffetre.html
Recent batches of color have been exceptionally bright and clean.
lissa.
http://www.cauldroncreations.com/pasteleffetre.html
Recent batches of color have been exceptionally bright and clean.
lissa.
- Sat Aug 30, 2003 6:09 pm
- Forum: Techniques and Tools
- Topic: Hotline's new Primo Primer.. anyone using?
- Replies: 1
- Views: 2620
- Thu Aug 28, 2003 1:21 pm
- Forum: Business Topics
- Topic: Interesting info wrt Credit Cards....at least new to me
- Replies: 24
- Views: 24725
When I had a retail shop, my merchant account charged me MORE when someone used a debit card than if they charged on credit. That reserve that places do actually worked to my advantage. While in Orlando a few weeks ago I had my wallet stolen, a huge headache and a very worrisome event. But...we had ...
- Tue Aug 26, 2003 5:31 pm
- Forum: Photos and Stuff
- Topic: A retro piece for the older folks
- Replies: 15
- Views: 17300
- Tue Aug 26, 2003 11:01 am
- Forum: Techniques and Tools
- Topic: Intriguing surface defect
- Replies: 7
- Views: 7432
This was happening to me a lot, more with certain colors, on both ground and unground edges, obviously a lot worse with the ground edges. I have found super spray to be helpful (and not grinding!). I don't know if you use anything like that but now I rarely get that haze line. I wondered if it had t...