Search found 6 matches

by Ron Evans
Wed Jan 16, 2013 11:16 am
Forum: Newcomer Forum
Topic: Fusing with metal
Replies: 6
Views: 20771

Re: Fusing with metal

Thanks to all who responded. I will have to try several of those ideas.
by Ron Evans
Tue Jan 15, 2013 9:45 pm
Forum: Newcomer Forum
Topic: Kiln recommendation?
Replies: 5
Views: 16066

Re: Kiln recommendation?

I have just purchased a JenKen 15/6 which I like very much. If I had it to do again though I would probably try to get a bigger one. The controller is what sold me. Easy to use and the results have been great so far. Have fun! :)
by Ron Evans
Tue Jan 15, 2013 9:41 pm
Forum: Newcomer Forum
Topic: Fusing with metal
Replies: 6
Views: 20771

Fusing with metal

I have read that it is possible to fuse metal between two pieces of compatible glass. What type of metals can be used and what are specific procedures that must be adhered to? Thank you
by Ron Evans
Mon Dec 17, 2012 10:43 am
Forum: Newcomer Forum
Topic: Draping Problem
Replies: 10
Views: 26671

Re: Draping Problem

I did all the above and especially the peeking. I actually did a quick freeze at the 1225 degree temp and started the cool down almost immediately after the kiln reached the top temp. Skipped the soak time at the top and continued on with the annealing. Came out really good! Thanks for everyone's ex...
by Ron Evans
Sun Dec 16, 2012 12:39 pm
Forum: Newcomer Forum
Topic: Draping Problem
Replies: 10
Views: 26671

Re: Draping Problem

Thank you. I will try that next. Not sure how low to go since the top temp in the original program is 1280, but will try something like 1225 and see what happens. :)
by Ron Evans
Sun Dec 16, 2012 10:25 am
Forum: Newcomer Forum
Topic: Draping Problem
Replies: 10
Views: 26671

Draping Problem

I am new to warm glass and have a question about draping over a flower mold. I have a problem with the glass closing around the mold instead of staying open like I see in the glass stores. I have tried lowering the hold time at the top end by 50% but still did not work. Any ideas? Thanks