Postby Kathleen Ash » Tue Jul 06, 2021 9:33 am

Hello, I have not been able to find an answer and I'm hoping the forum can help: I am in the process of making a pate de verre box. The folks at Bullseye said that I would be able to use straight Hydrocal for my plaster mold. In Boyce Lundstrom's book he said to take the mold to 1200 degrees to burn out the wax that was left after steaming. The lid of my push mold ended up with edge cracking and the bowl part of the mold had several hairline cracks. I patched them up, wired the circumference and am hoping for the best. The test box looks pretty good in the kiln, but it's still at 1000. So my question is two part: Do I have to mix in silica flour with Hydrocal to prevent cracking? Is it OK to leave a waxy film on the inside of the mold and avoid firing the mold pre-filling? Thanks in advance! Kathleen

Steph Mader
Posts: 59
Joined: Tue Mar 11, 2003 1:45 am
Location: Freeland, WA
Contact:

Re: Hydrocal Hell

Postby Steph Mader » Mon Dec 13, 2021 8:02 pm

Hi Kathleen,
Yes, mix at least 50% silica flour with the hydrocal to make casting investment. It helps to add some chopped fiberglass too, to help hold everything together. Hydrocal by iteself can't handle the heat of the kiln and will break down and fail. Good luck!
Steph


Post Reply

Return to “Kiln Casting”

Who is online

Users browsing this forum: No registered users and 6 guests

Warm Glass

2575 Old Glory Road, Suite 700
Suite 700
Clemmons, NC 27012
Phone: (336) 712 8003
Email: wg@warmglass.com