I have a couple unopened samples of Zircar's Mold Mix 6, and they are almost rock solid. Has anyone tried to reconstitute this material with a little water and perhaps a blender? According to Zircar, it might not be worth the effort. I want to paint some on a mold made from Zircar sheet material, for a better texture and finish. Thanks.
Nikki
twin vision glass
Posts: 570
Joined: Thu Apr 29, 2004 12:55 am
Location: Invermere,B.C. Canada
Contact:

Re: Mold Mix 6

Post by twin vision glass »

I think I am sad to say that it would not be good . So sorry to break the bad news. It is SOOO wonderful when it is new and like thick cream
Give out Free Hugs!
website: http://www.twinvision.fusedglassartists.com
twin vision glass
Posts: 570
Joined: Thu Apr 29, 2004 12:55 am
Location: Invermere,B.C. Canada
Contact:

Re: Mold Mix 6

Post by twin vision glass »

Give out Free Hugs!
website: http://www.twinvision.fusedglassartists.com
Nikki ONeill
Posts: 169
Joined: Mon Mar 10, 2003 11:55 am
Location: Silver Spring, MD
Contact:

Re: Mold Mix 6

Post by Nikki ONeill »

Thank You Leslie for the wonderfully presented video. Clear, excellent instructions. I want to mention that I took my rock solid sample and immersed it in water for a day and it became workable. Mixing with a hand mixer made it creamy again. I hope the fibers are still in good shape!
twin vision glass
Posts: 570
Joined: Thu Apr 29, 2004 12:55 am
Location: Invermere,B.C. Canada
Contact:

Re: Mold Mix 6

Post by twin vision glass »

Well that is great. Let us know how it works for you. Try a small cast piece first perhaps open face . Les
Give out Free Hugs!
website: http://www.twinvision.fusedglassartists.com
Nikki ONeill
Posts: 169
Joined: Mon Mar 10, 2003 11:55 am
Location: Silver Spring, MD
Contact:

Re: Mold Mix 6

Post by Nikki ONeill »

Good idea. thanks Leslie!