Stupid question time--what is the point in "curing" a freshly kiln washed shelf? I can't see why preheating a fully dry shelf before using it at fusing temps is worth doing. What am I missing here?
Deb
-
jim simmons
- Posts: 478
- Joined: Sun Mar 09, 2003 10:37 pm
- Location: Hillsboro Oregon
- Contact:
Re: Kiln wash curing?
You are not missing anything if the shelf is drydaffodildeb wrote:Stupid question time--what is the point in "curing" a freshly kiln washed shelf? I can't see why preheating a fully dry shelf before using it at fusing temps is worth doing. What am I missing here?
Jim
-
daffodildeb
- Posts: 125
- Joined: Mon Jul 28, 2003 3:48 am
- Location: Hot Springs Village, AR
i have never prefired my kiln washed boards or molds, never used paper, and have never gotten a bubble under the glass. i have gotten bubbles between the layers of glass, but that isn't attributable to the wash.SAReed wrote:Uncured kiln wash can give off gases that will cause big bubbles
Stacey (who has had her share of big bubbles)
I've never cured the kiln wash in a mold since it has air holes.
I was making a platter that because of the design a bubble would form in the center. When using an un-cured kiln wash shelf the bubble was large, when using cured, it was small, more of an indentation.
I was making a platter that because of the design a bubble would form in the center. When using an un-cured kiln wash shelf the bubble was large, when using cured, it was small, more of an indentation.
Last edited by SAReed on Thu Oct 09, 2003 6:12 pm, edited 1 time in total.
Stacey
-
daffodildeb
- Posts: 125
- Joined: Mon Jul 28, 2003 3:48 am
- Location: Hot Springs Village, AR
A kiln shelf improperly dried (even in Arizona) will cause large steam bubbles to form between the bottom layer of glass and the shelf. You can get around the pre-drying by holding the firing at ~500°F for at least 30 minutes. This will not work if the shelf goes in damp. If the piece is very large (bigger than 14” in diameter) you will need to hold for a longer time period or pre-drying the shelf.
Tim
Tim
-
rosanna gusler
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
i have never pre dried shelves. i do not believe that there is any water left anywhere in the kiln by the time glass softens. i do believe that damp kiln wash makes a really good seal and can trap air. i put damp shelves in all the time . i do a 20 min hold at around 1100F. i have never gotten a bubble under the glass. rosanna
I was getting my bubbles with dried shelves, but not cured. I would put the kiln wash on, let dry a day or two, then fuse. Now I put the kiln wash on, let dry, then pre-fire. I don't know if I have to let it dry before I pre-fire, but I have a good thing going right now and I don't want to mess it up. 
Stacey
-
jim simmons
- Posts: 478
- Joined: Sun Mar 09, 2003 10:37 pm
- Location: Hillsboro Oregon
- Contact:
I have 2 shelves. I leave one on top of my kiln when I am doing a firing, and only take it off when I am ready to use it. Using BE kiln shalves, I have also never had a bubble under the glass. And I live just outside of Portland Orygun :>)Carol wrote:Um, I'm noticing that everyone who doesn't pre fire tends to live in hot, dry parts of the US. In rainier or more humid locations, it is less likely the kiln wash will dry completely in a reasonable period of time.
Jim