Artista glass compatibility
Moderators: Brad Walker, Tony Smith
Artista glass compatibility
Anyone know the CoE of the Artista glass described here?
http://www.schott.com/uk/english/produc ... tista.html
Is any of the Artista range compatible with BE CoE 90?
TIA
			
			
									
						
							http://www.schott.com/uk/english/produc ... tista.html
Is any of the Artista range compatible with BE CoE 90?
TIA
It ain't where you're from, it's where you're at!
			
						Artista is 90 COE, like BE, and compatible with it. Also with Uroboro, but my supplier said that the test is wanted. Annealing like BE. I don't like this type of glass: it is very hard( behaves like Float), at the same piece with BE the edges stay still sharp when the BE is already soft. Occasionaly I have  a work of BE+Artista in my kiln just now. It will take the couple of days to send you a photo, if you want. 
Anna.
			
			
									
						
										
						Anna.
- 
				Jan de Jong
- Posts: 114
- Joined: Sun Mar 09, 2003 3:31 pm
- Location: The Netherlands
Artista glass compatibility
Hi,
I use CLEAR Artista as base for BE, with good results (and cheaper !)
Further I think (so I don't say it is) the clear Artista is good for 1 layer projects. I did make a IceCrystal with only 1 layer and not the effect as by BE with one layer (sorry, did forget the name: the glass is going to the inside between the edges)
Jan
			
			
									
						
										
						I use CLEAR Artista as base for BE, with good results (and cheaper !)
Further I think (so I don't say it is) the clear Artista is good for 1 layer projects. I did make a IceCrystal with only 1 layer and not the effect as by BE with one layer (sorry, did forget the name: the glass is going to the inside between the edges)
Jan
- 
				Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
I believe that Artista is a cousin to the glass called GNA in the US. Lundstrom describes an interesting technique for making pate de verre hollow vessels using GNA and BE.  You need frit made with both glasses and you line the sides of a mold with a mixture of both frits.  The Be softens before the GNA so the GNA holds the matrix in place.  The BE provides the "glue" to hold it all together.  If fired properly, the glass will remain on the sides of the mold without falling down and you can make a vessel like a glass or a vase shape. They have the same expansions but very different viscosities.  Annealing must consider both glasses.
			
			
									
						
							Bert 
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
			
						Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Thanks folks.
The reason I'm considering Artista is to use it as a lid to cover BE elements. I'm looking at using 6mm clear Artista, because of price & availability.
Plus it's an excuse to take a trip to Deutschland and check if the beer quality is as good as it was 10 years ago and the missus can check the January sales.
Phil Isaac sent me a fantastic link to a comparison table showing characteristics & properties of clear float glass, Bullseye, transparent Spectrum, Uroboros and Artista. Well worth a look and bookmarking, if you use any of these glass types...
http://www.a-m.de/englisch/lexikon/visk ... tafel3.htm
 
Studying the table, couple of points;
-the softening point of Artista is 720degC and BE is 677degC, hence the harder glass characteristics Anna mentioned. Maybe the glass is also less fluid and will need a longer soak at full fuse to give a nice radiused edge.
-the annealing ramp would stay the same; I usually start at 570degC through to 370degC for BE, adjusting the rate of cooling according to the thickness of the piece.
Any further thoughts or experience of the above would be greatly appreciated, thanks in advance.
Oh and Jan you're not alone, I also have other names. Most of which are not suitable here but most recently Birthday Boy. (50yrs a few weeks ago)
			
			
									
						
							The reason I'm considering Artista is to use it as a lid to cover BE elements. I'm looking at using 6mm clear Artista, because of price & availability.
Plus it's an excuse to take a trip to Deutschland and check if the beer quality is as good as it was 10 years ago and the missus can check the January sales.
Phil Isaac sent me a fantastic link to a comparison table showing characteristics & properties of clear float glass, Bullseye, transparent Spectrum, Uroboros and Artista. Well worth a look and bookmarking, if you use any of these glass types...
http://www.a-m.de/englisch/lexikon/visk ... tafel3.htm
Studying the table, couple of points;
-the softening point of Artista is 720degC and BE is 677degC, hence the harder glass characteristics Anna mentioned. Maybe the glass is also less fluid and will need a longer soak at full fuse to give a nice radiused edge.
-the annealing ramp would stay the same; I usually start at 570degC through to 370degC for BE, adjusting the rate of cooling according to the thickness of the piece.
Any further thoughts or experience of the above would be greatly appreciated, thanks in advance.
Oh and Jan you're not alone, I also have other names. Most of which are not suitable here but most recently Birthday Boy. (50yrs a few weeks ago)
It ain't where you're from, it's where you're at!
			
						- 
				Cheryl Wade
- Posts: 26
- Joined: Sun Mar 23, 2003 5:48 pm
- Location: Wales UK
Paul
I haven't had too much experience with fusing, I'm taking evening classes in stained glass including warm glass. I use Artista for fusing projects and had no problems combining it with dichroic (from CBS) and Spectrum 90CoE fusible. I haven't used it with regular BE but have recently experimented with BE irridescent and have had problems- stress every time and immediate cracking when the Artista, BE and dichroic pieces touch each other. I've fused at 830C and 840C (I know this is really too high for the BE irridescent but wanted to see what it looked like - not bad) with 10 min soaks and very conservative annealing time. I'm going to refire the last disaster at 815C to see if that will help. As usual, do lots of test pieces.
Cheers
Cheryl
			
			
									
						
										
						I haven't had too much experience with fusing, I'm taking evening classes in stained glass including warm glass. I use Artista for fusing projects and had no problems combining it with dichroic (from CBS) and Spectrum 90CoE fusible. I haven't used it with regular BE but have recently experimented with BE irridescent and have had problems- stress every time and immediate cracking when the Artista, BE and dichroic pieces touch each other. I've fused at 830C and 840C (I know this is really too high for the BE irridescent but wanted to see what it looked like - not bad) with 10 min soaks and very conservative annealing time. I'm going to refire the last disaster at 815C to see if that will help. As usual, do lots of test pieces.
Cheers
Cheryl
- 
				Brian and Jenny Blanthorn
- Posts: 353
- Joined: Mon Mar 10, 2003 5:25 pm
- Location: UK
- Contact:
This link from Phil Isaac is goodPaul Stevenson wrote:Thanks folks.
The reason I'm considering Artista is to use it as a lid to cover BE elements. I'm looking at using 6mm clear Artista, because of price & availability.
Plus it's an excuse to take a trip to Deutschland and check if the beer quality is as good as it was 10 years ago and the missus can check the January sales.
Phil Isaac sent me a fantastic link to a comparison table showing characteristics & properties of clear float glass, Bullseye, transparent Spectrum, Uroboros and Artista. Well worth a look and bookmarking, if you use any of these glass types...
http://www.a-m.de/englisch/lexikon/visk ... tafel3.htm
Studying the table, couple of points;
-the softening point of Artista is 720degC and BE is 677degC, hence the harder glass characteristics Anna mentioned. Maybe the glass is also less fluid and will need a longer soak at full fuse to give a nice radiused edge.
-the annealing ramp would stay the same; I usually start at 570degC through to 370degC for BE, adjusting the rate of cooling according to the thickness of the piece.
Any further thoughts or experience of the above would be greatly appreciated, thanks in advance.
Oh and Jan you're not alone, I also have other names. Most of which are not suitable here but most recently Birthday Boy. (50yrs a few weeks ago)
http://www.a-m.de/englisch/lexikon/visk ... tafel3.htm
If U digg arround the site there is lots of secret stuff
From
http://www.a-m.de/englisch/index.html
Look at site map -- glass
There r viscoty tables hidden in there somewhere
The company appears 2 sell Bornnitride n shuch
Brian

- 
				Brian and Jenny Blanthorn
- Posts: 353
- Joined: Mon Mar 10, 2003 5:25 pm
- Location: UK
- Contact:
Re: Artista glass compatibility
Paul Stevenson wrote:Anyone know the CoE of the Artista glass described here?
http://www.schott.com/uk/english/produc ... tista.html
Is any of the Artista range compatible with BE CoE 90?
TIA
I got this a year or so ago
Artista coe 94
Are they now saying this is changed I could not find any coe stuff on the site link
Below is from my personal Top Secret files
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
Yo 2 all in Spab Land
I have used desag antique 75 since about 1981
http://www.blanthorn.com/bowls/bowls_19 ... _large.htm
Its flat no bubbles not tend 2 devit ( bubbles R on interface )
Its transparant
Crushed up it dosent devit either
http://www.blanthorn.com/bowls/bowls_19 ... _large.htm
Watch out 4 some colour combinations
Orangy + blues I think give brown at interface
In antique 75 some darker colours R not as compat
I have not used Artista but I expect it 2 B the same but should B more compatabbabe
Heres some stuff from my top secret private archives
----- Original Message -----
From: Brian Blanthorn
To: Brian and Jenny Blanthorn
Sent: Monday, February 26, 2001 9:45 PM
Subject: COE DESAG IMERA MAGIRA
Hi All added coe of Imera
If I have made error please tell
Changed all coe to 10 - 7
desag 75 is now Magera ( in USA its GNA )
unfortunately and this is BAD Magira GNA and Artista has the same pattern a very slight sort of wavy brushed pattern
Why they have not distinguished them is beyond me but then what do I know
XXXXXXXXXXXXXXXXXXXXXXXXXXXXXXX
Further to the information that you sent to me from the web-site and our subsequent telephone conversations I am pleased to forward the details that Schott Desag have responded with.
Co-efficient of expansions
Imera 90 - 96 a flat float type glass which is available in 9 colours but is not made compatable
Antique 75 Sold before 1990 90-96*10-7K-1
Magira 90-96*10-7K-1
Artista 94*10-7K1
"Artista is a closer specified version of Magira. This closer specification guarantees the fuseability of the Artista colours with each other.
Antique 75 is the old name of Magira. It was/is never made to be compatible.
When people succeed in fusing some Magira colours it happens because they have made test and the coefficient was coincidentally the same.
The name of Magira in USA is GNA - German New Antique"
I do hope this addresses the main questions.
Regards
Cathy Salt
XXXXXXXXXXXXXXXXXXXXXXX
Brian again
all glass in approx 3 - 9 mm size 1600 x 1500 some bigger
http://www.schott.com/desag/english/products/index.html
magira / artista / imera
note glass sink Barabra
http://www.schott.com/english/company/ main site
All the best
Brian

- 
				Cheryl Wade
- Posts: 26
- Joined: Sun Mar 23, 2003 5:48 pm
- Location: Wales UK
Paul
Yes, Artista is hard; lower temps, whilst full fusing, leave the surface of the individual pieces raised; even at 830C they look like shiny wine gums - almost good enough to eat - or is that too good to eat?
I tried some more test pieces using two colours of BE irridescent, both irridescent side up and down, and flat (not textured) dichroic on a clear Artista base - disaster, stress on each edge. Also the dichoic seeped irregularly along the joins - not a pretty sight. Looking at the table you posted, it seems as if it might be incompatible viscosities. I haven't tried coloured Artista yet but will do so to see if it's just a problem with the clear; shouldn't think so but you never know.
Brian
Your work is gorgeous. If it's not a secret, how do you make the pebbles? Are they cast? In several layers? How do you get the metallic outer surfaces? Not that I'll attempt to make any, just drool over yours.
Cheers
Cheryl
			
			
									
						
										
						Yes, Artista is hard; lower temps, whilst full fusing, leave the surface of the individual pieces raised; even at 830C they look like shiny wine gums - almost good enough to eat - or is that too good to eat?
I tried some more test pieces using two colours of BE irridescent, both irridescent side up and down, and flat (not textured) dichroic on a clear Artista base - disaster, stress on each edge. Also the dichoic seeped irregularly along the joins - not a pretty sight. Looking at the table you posted, it seems as if it might be incompatible viscosities. I haven't tried coloured Artista yet but will do so to see if it's just a problem with the clear; shouldn't think so but you never know.
Brian
Your work is gorgeous. If it's not a secret, how do you make the pebbles? Are they cast? In several layers? How do you get the metallic outer surfaces? Not that I'll attempt to make any, just drool over yours.
Cheers
Cheryl
- 
				Brian and Jenny Blanthorn
- Posts: 353
- Joined: Mon Mar 10, 2003 5:25 pm
- Location: UK
- Contact:
ThanksCheryl Wade wrote:Paul
Yes, Artista is hard; lower temps, whilst full fusing, leave the surface of the individual pieces raised; even at 830C they look like shiny wine gums - almost good enough to eat - or is that too good to eat?
I tried some more test pieces using two colours of BE irridescent, both irridescent side up and down, and flat (not textured) dichroic on a clear Artista base - disaster, stress on each edge. Also the dichoic seeped irregularly along the joins - not a pretty sight. Looking at the table you posted, it seems as if it might be incompatible viscosities. I haven't tried coloured Artista yet but will do so to see if it's just a problem with the clear; shouldn't think so but you never know.
Brian
Your work is gorgeous. If it's not a secret, how do you make the pebbles? Are they cast? In several layers? How do you get the metallic outer surfaces? Not that I'll attempt to make any, just drool over yours.
Cheers
Cheryl
On my web site there is a bio info which has some method info
In adition I do chat about most of the methods I use on the board
If U look em all up U will know more than I do
In brief the opalecent stuff is 4mm glass laminated in blocks in simple moulds
Fuzed then sawn /ground / polished
Some getting big now
About 18 " x 10 " 21 lb or so being 70 layers or so
Fired up very slow
Currently working on 24" slab saw so should get em bigger n easier
The opalecent effect is internal usually
Top secret, hence our fortified Island location , n underground lab complex
Brian