Oversprays on 3mm Clear Float: Spray A vs. Borax

Post by susan fancy »

When I use spray A on 3 mm clear float glass, it leaves a very slight haze in the top layer with a mottling effect from the spray pattern. I've tried applying different ways (airbrush, mouth sprayer, etc) and tried different drying periods, and also tin side down. I only see the haze when looking through the glass in stronger light.

Is anyone familiar with this? Way to correct it or the nature of the beast?

Thanks!
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: Oversprays on 3mm Clear Float: Spray A vs. Borax

Post by Bert Weiss »

susan fancy wrote:When I use spray A on 3 mm clear float glass, it leaves a very slight haze in the top layer with a mottling effect from the spray pattern. I've tried applying different ways (airbrush, mouth sprayer, etc) and tried different drying periods, and also tin side down. I only see the haze when looking through the glass in stronger light.

Is anyone familiar with this? Way to correct it or the nature of the beast?

Thanks!
Try borax
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Kevin Midgley
Posts: 774
Joined: Mon Mar 10, 2003 11:36 am
Location: Tofino, British Columbia, Canada

Post by Kevin Midgley »

Three things to do: Get a good glass that doesn't scum up. Clean the glass well. Don't fire as hot. I never use overglaze. Kevin
rosanna gusler
Posts: 730
Joined: Mon Mar 10, 2003 2:22 pm
Location: wanchese north carolina
Contact:

Post by rosanna gusler »

spray a makes float look dingey (sp) when compared to borax. rosanna
Cynthia

Post by Cynthia »

Spray A has lead in it as well as a ground glass. Borax is a fluxing agent like lead, but wouldn't contain the glass particles. Switch to the borax and I expect your results will be better.
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Post by Bert Weiss »

Kevin Midgley wrote:Three things to do: Get a good glass that doesn't scum up. Clean the glass well. Don't fire as hot. I never use overglaze. Kevin
Kevin

I don't use borax on glass 3/8" and thicker. I am led to understand that the thinner glasses aree more prone to devit because of the ease of certain molecules to rise to the surface. The thicker glasses hold that stuff inside.

When I do use borax, it comes out crystal clear on float. I did a round of sushi plates made of 2 layers of 3/16" with borax. They came out shiny and bright.