bentonite for sand casting
Moderators: Brad Walker, Tony Smith
-
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
bentonite for sand casting
I have read here that bentonite can be mixed with sand as an alternative to dry plaster. I have had great results using olivine sand and plaster.
i was speaking with a foundry guy today who told me that he thought that an olivine/bentonite mix would need 5% water to work right. he thought that the water was needed to disperse the bentonite around the sand.
I don't picture that the moist pac would be good to use for kiln fired glass.
Can anybody tell me about how they use the bentonite for kiln casting. Is it good as a seperator dusting?
i was speaking with a foundry guy today who told me that he thought that an olivine/bentonite mix would need 5% water to work right. he thought that the water was needed to disperse the bentonite around the sand.
I don't picture that the moist pac would be good to use for kiln fired glass.
Can anybody tell me about how they use the bentonite for kiln casting. Is it good as a seperator dusting?
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
- Posts: 730
- Joined: Mon Mar 10, 2003 2:22 pm
- Location: wanchese north carolina
- Contact:
,,,,,,,,,,,,,,thanks robert, would you kindly send the info on what berteil v. does with thisRobert Middlestead wrote:Bert
I did a casting workshop with Berteil V. some years ago and have his sand mixture on paper - will post if you need it but he adds only 5
percent bentonite well mixed into the sand .
Robert
is the water in the mix for the molten glass used to prevent the side wall of the sand from caving in,,,,,,if a persons uses a sheet of glass, what keeps the tops of any peaks from becoming flat
once the process is complete, is there ever any need for cold working, is there any sticking
thanks
rodney
-
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
I too took sand casting with Bertil V. and Paul M. Kiln casting is a different animal.Robert Middlestead wrote:Bert
I did a casting workshop with Berteil V. some years ago and have his sand mixture on paper - will post if you need it but he adds only 5
percent bentonite well mixed into the sand .
Robert
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
-
- Posts: 260
- Joined: Thu Mar 13, 2003 8:26 pm
- Location: Atlanta
Robert,Robert Middlestead wrote:Bert
I did a casting workshop with Berteil V. some years ago and have his sand mixture on paper - will post if you need it but he adds only 5
percent bentonite well mixed into the sand .
Robert
I'm interested in what Berteil uses for the negative forms in his pieces. This is for hot casting. He pre-forms some sand mixture, often into heads and faces, and places them into the bottom of molds to make a negative space. Do you know what he uses for this?
We tried using sodium silicate bonded sand last summer at Pilchuck but it turned into hard rock during annealing. The word was that his negative forms turn to powder during annealing. I've heard he may use some kind of oil bonded sand from the UK. Are you familiar with this?
Thanks, ch
-
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Charlie
We used 2 meshes of olivine sand and bentonite. I don't remember the percentages, but I probably have the notes at home (where I'm not).
First you sift the sand in to a box so that it is lofty. Then he presses in his large form, like the boat hull. Then he presses in objects. You could use anything from plastic toys to wooden carvings... Finally the mold is coated with graphite or carbon from an acetylene torch in places where he doesn't want the sand to stick. No carbon where he wants it to stick. Then molten glass is poured in, using a team of ladlers. As the mold fills up, he drops in objects made of compatible glass or copper foil. The whole box,sand and glass goes in to the annealer...
We used 2 meshes of olivine sand and bentonite. I don't remember the percentages, but I probably have the notes at home (where I'm not).
First you sift the sand in to a box so that it is lofty. Then he presses in his large form, like the boat hull. Then he presses in objects. You could use anything from plastic toys to wooden carvings... Finally the mold is coated with graphite or carbon from an acetylene torch in places where he doesn't want the sand to stick. No carbon where he wants it to stick. Then molten glass is poured in, using a team of ladlers. As the mold fills up, he drops in objects made of compatible glass or copper foil. The whole box,sand and glass goes in to the annealer...
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Berteils small negative pieces ie little figures do turn to powder after the
process but we didn`t make any during the class . He said someone
makes them for him in Sweden . Berteil has the luxury of working for
a large glass production co. so has many helpers . Someone emailed
me for his sand mix . He gave us two versions :
1/4 old sand
1/4 60 mesh
1/2 90 mesh
5 percent bentonite
Second version :
equal parts - 80 mesh and 120 mesh sand with 5 percent bentonite
A lot of time is spent mixing this stuff . He emphasized that .
process but we didn`t make any during the class . He said someone
makes them for him in Sweden . Berteil has the luxury of working for
a large glass production co. so has many helpers . Someone emailed
me for his sand mix . He gave us two versions :
1/4 old sand
1/4 60 mesh
1/2 90 mesh
5 percent bentonite
Second version :
equal parts - 80 mesh and 120 mesh sand with 5 percent bentonite
A lot of time is spent mixing this stuff . He emphasized that .
-
- Posts: 773
- Joined: Mon Mar 10, 2003 11:36 am
- Location: Tofino, British Columbia, Canada
Get an odd-job (that isd what it is called) Canadian made cement mixer for mixing mold materials. It is a small plastic barrel with baffles inside that is designed for a full bag of redimix cement. You dump in your materials lock on the lid and roll it across the floor. Works fast. They are under $40 Cdn. Kevin in Tofino
80-10-10 sand/bent/water but you need to mull the hell out of it - I use my truck to run it over a few times. You also should use a steel frame and pack it with a ram. The mold has to be heated to 200 for about 8 hours to get all the water out before you charge or you will have big bubbles in your glass. Lots of torching helps for release.
http://home2.nikonnet.com/servlet/com.a ... emberguest