Hi There...
A mold I was preparing for slumping just broke in two pieces as it was drying in the kiln and I've no idea why - can anyone help?
I had re-applied kiln wash to my shelf and dried it in the kiln to 500 and it was cooling but by no means cold.
Having sanded and kiln washed the mold I put it in the kiln to dry on top of the kiln shelf. When the temperature reached 460 I heard a thump and when I looked I saw that the mold had broken into two pieces, the crack was more or less straight through the middle. The mold was a bowl 12inch in diameter and about 4 inches deep.
Best regards
Linda
Broken Mold
Moderators: Brad Walker, Tony Smith
-
Linda Denli
- Posts: 21
- Joined: Wed Aug 27, 2003 2:58 pm
- Location: London, UK
Broken Mold
Linda from London
-
Lisa Allen
- Posts: 212
- Joined: Sun Mar 09, 2003 3:23 pm
- Location: Memphis, TN
- Contact:
Sounds like the mold thermal shocked. A lot of my molds come with a little note saying not to heat at more than 250dph. If you heated it afap to 500, that might be your culprit.
Lisa
Lisa
Lisa Allen
http://www.lisa-allen.com
Today's mighty oak is just yesterday's nut that held its ground.
http://www.lisa-allen.com
Today's mighty oak is just yesterday's nut that held its ground.