Relief Fusing
Moderators: Brad Walker, Tony Smith
Relief Fusing
In the latest Glass Craftsman, Robin Evans wrote an article on glass mosaic and she says you should do a fast relief fuse of the dichroic strips. Does anyone know the specifics of how to do a relief fuse and at that a fast one? This is a new term to me.
-
Jackie Beckman
- Posts: 475
- Joined: Sun Mar 09, 2003 5:01 pm
- Location: Arizona
- Contact:
Hi Lori:
Jackie nailed it - in the article I mentioned various stages and a relief fuse to me has more rounded edges than a tack fuse. Here's my firing schedule for a fast relief fuse for the up to 8" long x 1/2" wide dichroic strips you see on the piece in the article:
800 DPH to 1100
Hold 15 min
600 DPH to 1250
Hold 20 min
600 DPH to 1410
Hold 10 min
AFAP to 960
Hold 30 min
200 DPH to 750
No hold
I get nicely rounded edges and a surface shift on the dichroic that I like using the above. Have fun.
RobinE
Jackie nailed it - in the article I mentioned various stages and a relief fuse to me has more rounded edges than a tack fuse. Here's my firing schedule for a fast relief fuse for the up to 8" long x 1/2" wide dichroic strips you see on the piece in the article:
800 DPH to 1100
Hold 15 min
600 DPH to 1250
Hold 20 min
600 DPH to 1410
Hold 10 min
AFAP to 960
Hold 30 min
200 DPH to 750
No hold
I get nicely rounded edges and a surface shift on the dichroic that I like using the above. Have fun.
RobinE