I just bought a cple of new stainless floral former and Hitemp1800
Sprayed them, fired them to 700.
Put glass on when cold, set in kiln with some that I have had for years, the glass on new former stuck and broke, older ones were fine.
Any ideas?
tks
stainless floral former
Moderators: Brad Walker, Tony Smith
-
Bert Weiss
- Posts: 2339
- Joined: Tue Mar 11, 2003 12:06 am
- Location: Chatham NH
- Contact:
Re: stainless floral former
poor coverage of the BN? Sandblast the steel clean and try regular kiln wash, a few coats.
Bert
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Re: stainless floral former
thankyou
will try
will try
-
bob proulx
- Posts: 186
- Joined: Tue Dec 29, 2009 7:13 pm
- Location: Nahant Massachusetts
- Contact:
Re: stainless floral former
I agree with Bert, sandblast and use kiln wash.
Bob
Bob
-
Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
Re: stainless floral former
I always put a slightly oversize disc of fiber paper over the end of the floral former. Just a bit paranoid about the glass getting stuck.
Tony
Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..." Scott Berkun