hypothetically , if a project was not sufficiently annealed, is it possible to reheat to anneal temp and redo the anneal ?
thanks Stef
annealing 96 question
Moderators: Brad Walker, Tony Smith
-
Joe Wokovich
- Posts: 32
- Joined: Tue Sep 25, 2007 1:57 pm
- Location: Florissant, MO (@ St. Louis, MO)
Re: annealing 96 question
Shouldn't be a problem. Just go really slow on the heat up. Then use your regular schedule for finishing the firing.
Joe
Joe
“If you tell me, I will forget.
If you show me, I will remember.
If you let me do it, I will understand."
And then tomorrow I can start all over again
If you show me, I will remember.
If you let me do it, I will understand."
And then tomorrow I can start all over again
Re: annealing 96 question
25 degreesC (77F ) be slow enough?
-
Rick Wilton
- Posts: 273
- Joined: Sat Oct 25, 2003 8:18 pm
- Location: Calgary, Canada
- Contact:
Re: annealing 96 question
how big? How thick? full fused or tack fused?
No easy answer to that question.
Good Luck
No easy answer to that question.
Good Luck
Rick Wilton
-
twin vision glass
- Posts: 570
- Joined: Thu Apr 29, 2004 12:55 am
- Location: Invermere,B.C. Canada
- Contact:
Re: annealing 96 question
Don't forget to go above anneal and hold for abit before you go back down to anneal to make sure the inside of glass is same temp for even anneal. (I have taken a larger piece back up to 1100 F. but because it was an inch thick I went toooo quickly and broke it, THEN went 50 deg per hour back up to full fuse and it all went back together so nicley), so slow down to 50 deg. per hour just like suggested above and it will help to even heat everything as well. Les
Give out Free Hugs!
website: http://www.twinvision.fusedglassartists.com
website: http://www.twinvision.fusedglassartists.com
Re: annealing 96 question
1/2"(12mm) thick,
12" ( 30cm) round.
Slump ( into sand) prog was:
Farenheit;
300/1000/20
570/1380/60
AFAP/1000/45
75/970/90
75/900/15
130/750/10
Celcius;
150/540/20
300/750/60
AFAP/540/45
25/520/90
25/485/15
55/400/10
I thought this ramp down would be slow enough to anneal but seems not.
2 of the discs seem fine, 1 has broken through the centre while I was scrubbing the sand off it, 1 is still in the kiln on the sand so I thought I might try taking it up again and adding an extra hour soak at 900 (485)
So the questions are ...
how fast to go up ( to 1000(540) )
and am I ramping down slow enough
Am I soaking at the right temps??
cheers Stef
12" ( 30cm) round.
Slump ( into sand) prog was:
Farenheit;
300/1000/20
570/1380/60
AFAP/1000/45
75/970/90
75/900/15
130/750/10
Celcius;
150/540/20
300/750/60
AFAP/540/45
25/520/90
25/485/15
55/400/10
I thought this ramp down would be slow enough to anneal but seems not.
2 of the discs seem fine, 1 has broken through the centre while I was scrubbing the sand off it, 1 is still in the kiln on the sand so I thought I might try taking it up again and adding an extra hour soak at 900 (485)
So the questions are ...
how fast to go up ( to 1000(540) )
and am I ramping down slow enough
Am I soaking at the right temps??
cheers Stef
Re: annealing 96 question
Here are the suggested firing and annealing recommendations from System 96:
http://www.system96.com/Pages/ThickFiringGuideF.html
I would follow the 1 inch recommendation since you are firing on the sand bed.
Barb
http://www.system96.com/Pages/ThickFiringGuideF.html
I would follow the 1 inch recommendation since you are firing on the sand bed.
Barb
Re: annealing 96 question
thanks Barb,
that makes sense... my thinking was stuck in a groove... I thought I had the correct firing prog from when I did this about a year ago but I must have lost the right page with the longer program from my folder. It just didn't connect with my brain that the anneal soak was too short.
(Note to self; ... tidy folder & studio.)
Now I need to re anneal the discs which haven't broken.
Any idea on how fast/what temp I should reheat at ??
Any advice from anyone is much appreciated.
stef
I have tried to upload a photo of what I am doing but It tells me that the file is invalid... What does that mean?
I'm not very clever with computers!
that makes sense... my thinking was stuck in a groove... I thought I had the correct firing prog from when I did this about a year ago but I must have lost the right page with the longer program from my folder. It just didn't connect with my brain that the anneal soak was too short.
(Note to self; ... tidy folder & studio.)
Now I need to re anneal the discs which haven't broken.
Any idea on how fast/what temp I should reheat at ??
Any advice from anyone is much appreciated.
stef
I have tried to upload a photo of what I am doing but It tells me that the file is invalid... What does that mean?
I'm not very clever with computers!
Re: annealing 96 question
I'd go up at 50 dph (or slower) to 1000 degrees, then come back down through the recommended annealing schedule... Good Luck!
Barb