Opaque Enamel Question

Post by DaveInSoKona »

I got a bunch of the Opaque Enamel powders and mixed them with the water friendly medium and fired to 1328 degrees. Two problems:

1. They don't come out shiny like the samples look even with Super Spray.

2. Red is either burning off (mixed with yellow to make orange) or coming our black no mixing, pure powder with medium.

Any ideas? Thanks.
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Re: Opaque Enamel Question

Post by Brock »

DaveInSoKona wrote:I got a bunch of the Opaque Enamel powders and mixed them with the water friendly medium and fired to 1328 degrees. Two problems:

1. They don't come out shiny like the samples look even with Super Spray.

2. Red is either burning off (mixed with yellow to make orange) or coming our black no mixing, pure powder with medium.

Any ideas? Thanks.
Matte enamels usually mean they haven't matured (got hot enough).
Reds burning out usually mean you went too hot. Hmmm . . .

What kind of enamels?
My memory is so good, I can't remember the last time I forgot something . . .
dan001
Posts: 32
Joined: Wed Oct 15, 2003 10:36 am
Location: Montreal

Post by dan001 »

If you are working with reusches, my best results were at 1250.

Dan
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: Opaque Enamel Question

Post by Bert Weiss »

Brock wrote:
DaveInSoKona wrote:I got a bunch of the Opaque Enamel powders and mixed them with the water friendly medium and fired to 1328 degrees. Two problems:

1. They don't come out shiny like the samples look even with Super Spray.

2. Red is either burning off (mixed with yellow to make orange) or coming our black no mixing, pure powder with medium.

Any ideas? Thanks.
Matte enamels usually mean they haven't matured (got hot enough).
Reds burning out usually mean you went too hot. Hmmm . . .

What kind of enamels?
I totally agree with that experience.
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
DaveInSoKona

Post by DaveInSoKona »

They are the "Fuse Master Lead-Free Opaque Enamels" from Fusion 1300-1500 firing range.