Once upon a time, there was a very imformative thread about this topic, but I think it's been lost. I'll ask again. Here's the scenario...

First layer: Clear glass blank as the base (say 8x8). Second layer: Something interesting in the middle in opal glass (say 4x4). Two inch opal border all around, in 2x6 pieces. All pieces fit together nice and tight. When it's full fused, I can see the lines where the border pieces have been butted against each other. How to I avoid getting these lines?

Thanks in advance for your advice.
The Hobbyist
Posts: 311
Joined: Sun Mar 09, 2003 7:09 pm
Location: Sun City West (NW Phoenix), AZ
Contact:

Re: Line shows on opal borders

Post by The Hobbyist »

"Flip and Fire"

Fire it face down. Flip it over and refire.

Jim
"With or without religion, good people can behave well and bad people can do evil; but for good people to do evil—that takes religion. " Steven Weinberg
haleybach
Posts: 75
Joined: Tue Sep 04, 2012 1:59 pm
Location: Austin TX

Re: Line shows on opal borders

Post by haleybach »

Angle the cuts so there is slight overlap. Kind of like a side ways miter cut if that makes any sense.
Tony Smith
Posts: 1037
Joined: Sun Mar 09, 2003 5:59 pm
Location: Massachusetts, USA
Contact:

Re: Line shows on opal borders

Post by Tony Smith »

Can you see the lines because the piece has thinned out at the joint? This can happen with two layers if the glass is on the thin side. Another possibility is that the glass is moving slightly during heat up. Damming the piece would prevent the glass from moving. Adding a third layer, or using a 6mm base glass along with damming should eliminate both problems.

Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..." Scott Berkun
Morganica
Posts: 1079
Joined: Mon May 19, 2003 6:19 pm
Location: Portland, OR
Contact:

Re: Line shows on opal borders

Post by Morganica »

All of the above, plus fire a bit hotter/longer. Opals, particularly the lighter colors, tend to be stiffer glass that needs more heatwork to flow and blend together. The problem is, getting the opals to flow means that the darker transparents, particularly black, will have been flowing for awhile, so they may start wavering.

That's why I sometimes prefire pale opals and whites and get them flowing, then go back and add in my darks in a second firing.
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com

"I wrote, therefore I was." (me)
Jerrwel
Posts: 129
Joined: Thu Feb 10, 2005 6:25 pm
Location: Charlotte, NC

Re: Line shows on opal borders

Post by Jerrwel »

Tony Smith wrote:Can you see the lines because the piece has thinned out at the joint? This can happen with two layers if the glass is on the thin side. Another possibility is that the glass is moving slightly during heat up. Damming the piece would prevent the glass from moving. Adding a third layer, or using a 6mm base glass along with damming should eliminate both problems.

Tony
CH Glass, have you seen Tony's work? He is the master of precisionhttp://www.blastedglass.com/newwork/img_1746.jpg. I'm always in awe when I look at his websitehttp://www.blastedglass.com/.
Jerry
CH Glass
Posts: 16
Joined: Sun Mar 21, 2010 3:43 pm

Re: Line shows on opal borders

Post by CH Glass »

Sorry I have been delinquent responding. Thank you very much for all your advice!