Bullseye Striker colors

Post by Havi »

I believe I heard somewhere that in order for the colors which are called strikers - to strike, one needs to get thru a particular process , making a hold at a particular temperature , about 1238 degrees.

Has anybody heard about it too? And what is the temperature I must go thru, for how long?

I'd be grateful For your response,

Many thanks,


Havi
Haviva Z
- - - - with a smile :)

"Speed comes from the Devil" - (an Arabic proverb)
Image
http://www.havivaz.com
Lynn Perry
Posts: 129
Joined: Sun Jun 08, 2003 5:27 pm
Location: East Tennessee

Re: Bullseye Striker colors

Post by Lynn Perry »

Havi, here is a link to a search of the Bullseye website about firing striker glass. Some of the colors require a slow firing for the color to fully appear:

http://www.bullseyeglass.com/search.htm ... ng+striker
Lynn Perry
Havi
Posts: 619
Joined: Wed Jul 02, 2003 6:01 am
Location: Israel
Contact:

Re: Bullseye Striker colors

Post by Havi »

Thanks Lynn!

I finally found the quotation on BE [perhaps it was on their educational video]


You have to hold 45 minutes at 1250 F - [677 centigrade] in order to 'strike' the striker colors.


many thanks again,


Havi
Haviva Z
- - - - with a smile :)