Newbie question: all other things being equal (using Bullseye glass) is a thicker piece more likely or less likely to crack during a slump? I'm trying to think it through and can see an argument for either way.
			
			
									
						
										
						- 
				rosanna gusler
 - Posts: 730
 - Joined: Mon Mar 10, 2003 2:22 pm
 - Location: wanchese north carolina
 - Contact:
 
Re: relationship between thickness and brittleness
it all depends on your schedule and set up. as a rule i think that the thicker the piece, the more conservative the heat up needs to be to achieve thermal evenivity. r.
			
			
									
						
							artist, owner of wanchese art studio, marine finisher
			
						- 
				DonMcClennen
 - Posts: 381
 - Joined: Sun Mar 09, 2003 9:09 pm
 - Location: Ontario
 
Re: relationship between thickness and brittleness
"Cracking during a slump" ?? have not had that problem in the last 20yrs. Low and Slow and as Rosanna said adjust for thickness. I think many or even most of the newbie problems are the result of too fast and too hot!  You didn't elaborate on you schedule or the thicknesses you are using so am unable to offer specific help.
			
			
									
						
							"The Glassman"
			
						- 
				Bert Weiss
 - Posts: 2339
 - Joined: Tue Mar 11, 2003 12:06 am
 - Location: Chatham NH
 - Contact:
 
Re: relationship between thickness and brittleness
The thicker the piece of glass the more difficult it is to heat evenly.  You must not get the surface too much hotter than the core.  So, slow down...
			
			
									
						
							Bert 
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
			
						Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Re: relationship between thickness and brittleness
"All things being equal" is a pretty sweeping assumption, but I'd say the thicker it is, the more likely you are to have cracking. There's simply more chance for a big difference between temperatures in the core of the piece and the surfaces.
I don't know that I'd characterize it as a brittleness problem, though.
			
			
									
						
							I don't know that I'd characterize it as a brittleness problem, though.
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
			
						Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
- 
				BadExampleMan
 - Posts: 28
 - Joined: Fri Nov 12, 2010 9:00 am
 - Location: Tel Aviv, Israel
 
Re: relationship between thickness and brittleness
Yeah, I know I didn't give any real details. I had two pieces that were virtually identical except one was 6mm thick and the other was 7.5mm; fired identically the thicker one cracked apart during a drape, and judging from the positions of the pieces it broke during the ramp up to process temp.
(Once I realized it had broken I aborted the program and opened the kiln. When the pieces were cool enough to handle I put them on a table, where they promptly exploded. First time that's happened to me, it was a little exciting.)
Anyway, thank you for the input.
			
			
									
						
										
						(Once I realized it had broken I aborted the program and opened the kiln. When the pieces were cool enough to handle I put them on a table, where they promptly exploded. First time that's happened to me, it was a little exciting.)
Anyway, thank you for the input.
- 
				Lauri Levanto
 - Posts: 270
 - Joined: Tue Mar 11, 2003 7:33 am
 - Location: Halikko, Finland
 
Re: relationship between thickness and brittleness
Somewhere I saw a value that the core and surface (or any two points in a piece) must be kept wthin 20C 36 F below the transition range. In annealing the delta is 5 C. There we are worried about permanent frozen in stress. In warming up we are worried about temporarily tolerable stress.
Above transition range the glass is supposed to 'give' and no stress may accumulate.
In draping -or pate de verre over acore it may tear apart, not break.
My 0.02€
-lauri
			
			
									
						
										
						Above transition range the glass is supposed to 'give' and no stress may accumulate.
In draping -or pate de verre over acore it may tear apart, not break.
My 0.02€
-lauri
- 
				Bert Weiss
 - Posts: 2339
 - Joined: Tue Mar 11, 2003 12:06 am
 - Location: Chatham NH
 - Contact:
 
Re: relationship between thickness and brittleness
I agree with Cynthia that there is a semantic issue. Brittle is not the best word. Stresses are cumulative. So if a piece has existing stress from a poor anneal or compatibility issues, and you add thermal shock stress, it will break. A well annealed more compatible piece might be able to withstand a bit more shock before it destructs.Morganica wrote:"All things being equal" is a pretty sweeping assumption, but I'd say the thicker it is, the more likely you are to have cracking. There's simply more chance for a big difference between temperatures in the core of the piece and the surfaces.
I don't know that I'd characterize it as a brittleness problem, though.
Bert 
Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
			
						Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions