Bending 2mm Stringer
Moderators: Brad Walker, Tony Smith
-
David Jenkins
- Posts: 174
- Joined: Wed Apr 29, 2009 10:35 pm
- Location: Cypress, Texas
Bending 2mm Stringer
I'd like to put about a 45 deg. bend in a short section of stringer, but I'd like to do it around about a 1" radius. I've tried using an alcohol burner to heat the glass, but the heat is so localized that the minute it's soft enough to bend the glass, it gets a bend radius of something approaching zero. Is there any way to get a gentle, large radius bend into the stringer?
Thanks.
Thanks.
Dave Jenkins
Glass at Harbor Gates
Cypress, TX
Glass at Harbor Gates
Cypress, TX
Re: Bending 2mm Stringer
Use a tea light, less heat, better control
Monika
Live is a Journey - Not a Destination
Live is a Journey - Not a Destination
-
Brad Walker
- Site Admin
- Posts: 1539
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: Bending 2mm Stringer
Slump it.
Re: Bending 2mm Stringer
Tea light works. Other thing with an alcohol burner is to hold it away from the flame a bit and keep it moving steadily. Let the weight of the stringer make the curve for you.
Cynthia Morgan
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
Marketeer, Webbist, Glassist
http://www.morganica.com/bloggery
http://www.cynthiamorgan.com
"I wrote, therefore I was." (me)
-
David Jenkins
- Posts: 174
- Joined: Wed Apr 29, 2009 10:35 pm
- Location: Cypress, Texas
Re: Bending 2mm Stringer
Thanks, all.
I think I'll try the slump idea first. Once I've found the right combination of heat, time, and distance between the supports to yield what I want, I should be able to turn out a lot of these in a very short time. Plus, that approach won't require as much manual dexterity as the others.
I'll have to put up with a catenary instead of a circular arc, but ... any port in a storm - right?
I think I'll try the slump idea first. Once I've found the right combination of heat, time, and distance between the supports to yield what I want, I should be able to turn out a lot of these in a very short time. Plus, that approach won't require as much manual dexterity as the others.
I'll have to put up with a catenary instead of a circular arc, but ... any port in a storm - right?
Dave Jenkins
Glass at Harbor Gates
Cypress, TX
Glass at Harbor Gates
Cypress, TX
-
Brad Walker
- Site Admin
- Posts: 1539
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: Bending 2mm Stringer
You can get a circular arc if you slump into the right shape, instead of just hanging from supports. Try carving a kiln brick to get the shape you want.David Jenkins wrote:I'll have to put up with a catenary instead of a circular arc, but ... any port in a storm - right?
-
David Jenkins
- Posts: 174
- Joined: Wed Apr 29, 2009 10:35 pm
- Location: Cypress, Texas
Re: Bending 2mm Stringer
Thanks, Brad.
I was just kidding - the catenary shape will work just fine. I'm really after a semi-uniform gentle curve, and once I get the slump parameters set, as well as the distance between the supports, I'll be able to turn them out in the volume that I need.
I was just kidding - the catenary shape will work just fine. I'm really after a semi-uniform gentle curve, and once I get the slump parameters set, as well as the distance between the supports, I'll be able to turn them out in the volume that I need.
Dave Jenkins
Glass at Harbor Gates
Cypress, TX
Glass at Harbor Gates
Cypress, TX
-
Brad Walker
- Site Admin
- Posts: 1539
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: Bending 2mm Stringer
"Catenary" -- which for some reason my spell checker says is not a word -- is one of my favorite words. According to Henry Halem's Glass Notes, it's the perfect curve for the arch of a home made glass furnace.David Jenkins wrote:the catenary shape will work just fine.
Now where did I leave that rope?
-
lorimendenhall
- Posts: 91
- Joined: Wed Apr 10, 2013 8:54 pm
- Location: Orange County, CA
- Contact:
-
David Jenkins
- Posts: 174
- Joined: Wed Apr 29, 2009 10:35 pm
- Location: Cypress, Texas
Re: Bending 2mm Stringer
The catenary is an Interesting function that describes the shape defined by a wire, chain, or rope, etc. suspended between two supports. It is given by:
y = a cosh (x/a)
where a is the distance between the two supports, and 'cosh' represents the hyperbolic cosine function.
(I just knew a math major would become useful sooner or later.
)
I'm not really sure that a piece of slumping glass in free space falls into a catenary or not - seems to me there would be some other variables at play: viscosity, COE, heat transfer velocity, etc. I was just trying to be a vocabulary show-off, I guess.
y = a cosh (x/a)
where a is the distance between the two supports, and 'cosh' represents the hyperbolic cosine function.
(I just knew a math major would become useful sooner or later.
I'm not really sure that a piece of slumping glass in free space falls into a catenary or not - seems to me there would be some other variables at play: viscosity, COE, heat transfer velocity, etc. I was just trying to be a vocabulary show-off, I guess.
Dave Jenkins
Glass at Harbor Gates
Cypress, TX
Glass at Harbor Gates
Cypress, TX
-
Brad Walker
- Site Admin
- Posts: 1539
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: Bending 2mm Stringer
Now there's a phrase I never thought I'd see on this board.David Jenkins wrote:and 'cosh' represents the hyperbolic cosine function.
I found a web page that discussed the difference between a parabola and a catenary: http://mathforum.org/library/drmath/view/65729.html The target audience was math students, but to me the most interesting part of the page was where the expert (Dr. Math, of course) says: "Once you have learned calculus, you will be able to see that the catenary is the solution to a differential equation that describes a shape that directs the force of its own weight along its own curve, so that, if hanging, it is pulled into that shape, and, if standing upright, it can support itself."
So of course slumped glass would fall into a catenary -- just don't get it too hot.
-
DonMcClennen
- Posts: 381
- Joined: Sun Mar 09, 2003 9:09 pm
- Location: Ontario
Re: Bending 2mm Stringer
for larger radii I drape rather than slump. A piece of pipe or any such shape... place (balance) stringer over.... add heat to stringer with blow torch.
"The Glassman"
Re: Bending 2mm Stringer
I've draped over pipe -- guess it was around 1.5" diameter, but in the kiln, not with a torch. I cut the stringer a little longer than I wanted, then trimmed the ends after firing.