Hello friends.

I did a fusing using Murano Glass coe 104

I created 15 Tiles -5mm clear + Murrine MIllefiori on . Some of they after fusing got some (cracks?) in the bottom while others have soome strange white scratches on the top.

I used BE thinfine.

Please can you understand what happened? can refuse ? can use Spray A on the top ?

thanks for support and collaboration

mike from italy

Image

Image





scratch on the top
thanks for sharing !

mike from italy


"secret of success?... passion & experience"

http://www.picturetrail.com/mikefromitaly
Bert Weiss
Posts: 2339
Joined: Tue Mar 11, 2003 12:06 am
Location: Chatham NH
Contact:

Re: 104 : cracks and scratches

Post by Bert Weiss »

It is hard to say. The lines on top appear to be mini starts that happened during the heatup and healed at the top. The cracks on the bottom may well be due to poor annealing. I don't see evidence of incompatibility.

Glass has a way of showing you what has happened to it throughout it's heating and cooling history. I doubt you can heal all that.
Bert

Bert Weiss Art Glass*
http://www.customartglass.com
Furniture Lighting Sculpture Tableware
Architectural Commissions
Marty
Posts: 865
Joined: Mon Mar 10, 2003 3:58 pm
Location: Maine
Contact:

Re: 104 : cracks and scratches

Post by Marty »

Sure looks like incompat. cracks around each mf (unless it's a photo artifact). No idea re the lines. Did you check with polarizing films?
jim simmons
Posts: 478
Joined: Sun Mar 09, 2003 10:37 pm
Location: Hillsboro Oregon
Contact:

Re: 104 : cracks and scratches

Post by jim simmons »

What Marty said.
Jim

Marty wrote:Sure looks like incompat. cracks around each mf (unless it's a photo artifact). No idea re the lines. Did you check with polarizing films?
Fiona Collins
Posts: 30
Joined: Sun Nov 17, 2013 9:10 am

Re: 104 : cracks and scratches

Post by Fiona Collins »

Hi Mike, what temp did you fuse to? Effetre clear (sheet and rod) generally has a lot of little bubbles and is quite textured, much harder to get clean than S96 or bullseye and some batches are just scummy. I scrub with a green scourer and dishwashing liquid, dry, then wipe down with cheap vodka. I also full fuse a bit hotter than recommended for 104 at S96 temps (anneal at 510C). Most 104 is only 104ish and can range from 100 - 108 and you will frequently see small cracks when using transparent and opals.
Barbara Elmore
Posts: 19
Joined: Wed Nov 19, 2003 5:47 pm
Location: State Road NC

Re: 104 : cracks and scratches

Post by Barbara Elmore »

Effetre 104 is a difficult glass to fuse. For me, it devitrifies horribly.

The commercially made murinni are not always compatible, and I can see the halos surrounding your murinni in the pictures. Clear signs of incompatibility.

Unfortunately, you cannot fix nor save these.

I am working on a project using Uroboros 104 now, and I am having compatibility problems with the red and mauve/light purple shifting COE's when firing in the kiln.
Thanks, Barbara Hale Elmore

"Good judgement comes from experience. Experience comes from bad judgement" Indian Proverb
mikefromitaly
Posts: 67
Joined: Thu Apr 03, 2003 7:47 am
Location: italy-sicily
Contact:

Re: 104 : cracks and scratches

Post by mikefromitaly »

hello and thanks for all your replies.

My target temp is 725C

never got devetrification neither stress with polaring films.

In my second fusing i clean more and better and results was eccellent.ok

mike
thanks for sharing !

mike from italy


"secret of success?... passion & experience"

http://www.picturetrail.com/mikefromitaly