Hello everybody
I found, the hard way, that if I anneal a piece which is 0.75", or thicker, it is safer for me to use annealing soak at 960 degrees, rather than the 'new' schedule to do the soak at 900 degrees.

Has anyone else noted this difference?

Many thanks,

Havi
Haviva Z
- - - - with a smile :)

"Speed comes from the Devil" - (an Arabic proverb)
Image
http://www.havivaz.com
Brad Walker
Site Admin
Posts: 1489
Joined: Fri Mar 07, 2003 9:33 pm
Location: North Carolina, USA
Contact:

Re: Annealing

Post by Brad Walker »

For what it's worth, Jody still anneals at 960F. The one time she tried at 900F she had the only annealing problem she's ever had.
Havi
Posts: 619
Joined: Wed Jul 02, 2003 6:01 am
Location: Israel
Contact:

Re: Annealing

Post by Havi »

Thanks again, Brad
Like i said.
I also had a lot of problems, once I annealed thicker, a bit thicker pieces at 900.

I wonder if others have also notices it....