Pot Melt Bubbles and Pits
Moderators: Brad Walker, Tony Smith
-
Mark Wright
- Posts: 49
- Joined: Mon Dec 13, 2010 12:43 pm
- Location: Raleigh, NC
Pot Melt Bubbles and Pits
Is there any way to prevent or get rid of the dozens of small bubbles and pits on the surface of a pot melt? After sandblasting and a second fusing it looks better but the pits are still there.
-
The Hobbyist
- Posts: 311
- Joined: Sun Mar 09, 2003 7:09 pm
- Location: Sun City West (NW Phoenix), AZ
- Contact:
Re: Pot Melt Bubbles and Pits
I always hold my melts at around 1500 F for about 45 min to an hour.
Jim "The Hobbyist"
Jim "The Hobbyist"
"With or without religion, good people can behave well and bad people can do evil; but for good people to do evil—that takes religion. " Steven Weinberg
-
Mark Wright
- Posts: 49
- Joined: Mon Dec 13, 2010 12:43 pm
- Location: Raleigh, NC
Re: Pot Melt Bubbles and Pits
My program:
1- 250/hr to 1000 hold 15
2- 250/hr to 1100 hold 15
3- 450/hr to 1685 hold 90
4- AFAP to 1520 hold 45
5- AFAP to 900 hold 60
6- 100/hr to 750 hold 15
1- 250/hr to 1000 hold 15
2- 250/hr to 1100 hold 15
3- 450/hr to 1685 hold 90
4- AFAP to 1520 hold 45
5- AFAP to 900 hold 60
6- 100/hr to 750 hold 15