Help with disaster fire

Post here with questions and topics relating to making glass jewelry.

Moderators: Brad Walker, Tony Smith

Post Reply
dianes
Posts: 5
Joined: Fri Aug 26, 2005 2:53 pm
Location: Fort Collins, CO

Help with disaster fire

Post by dianes »

Hi, we lived abroad for 7 years and I am just now returning to glasswork. My equipment and supplies were in a storage facility without heat or a/c. I fired my first pieces and they all migrated to the middle of the kiln shelf and fused together. I used the Basic 6 schedule from this site BASIC 6-Segment Firing Schedules.
http://system96.com/Resources/FiringGuideFahrenheit.pdf with System 96 glass. I suspect the temp was too high but fear there might be other contributing factors.

I used Thinfire shelf paper that no longer looks white from being in storage so long. It looks beige. Does shelf paper deteriorate?

I used to fire my kilns in my kitchen but have room in the garage in our new house. It was colder (low of 40 F0 and rainy when I fired. Does the garage need to be heated?

Thanks in advance for your kind assistance.

Diane
Attachments
FullSizeRender.jpg
FullSizeRender.jpg (31.33 KiB) Viewed 165617 times
The Hobbyist
Posts: 311
Joined: Sun Mar 09, 2003 7:09 pm
Location: Sun City West (NW Phoenix), AZ
Contact:

Re: Help with disaster fire

Post by The Hobbyist »

The old version of thinfire would shrink and curl up. Which may be the cause of your problem since your pieces are small.

Jim "The Hobbyist"
"With or without religion, good people can behave well and bad people can do evil; but for good people to do evil—that takes religion. " Steven Weinberg
Vonon
Posts: 197
Joined: Fri Mar 10, 2006 6:32 pm
Location: East Tennessee

Re: Help with disaster fire

Post by Vonon »

Is there a chance your shelf was stored in such a way that may have allowed it to warp slightly?
Vonon
jim simmons
Posts: 478
Joined: Sun Mar 09, 2003 10:37 pm
Location: Hillsboro Oregon
Contact:

Re: Help with disaster fire

Post by jim simmons »

Also, you might want to weigh down the edges/corners with some kind of kiln furniture.
This will keep it from curling so much.
The other Jim
dianes
Posts: 5
Joined: Fri Aug 26, 2005 2:53 pm
Location: Fort Collins, CO

Re: Help with disaster fire

Post by dianes »

Thanks JIM. I will check my self. The kiln furniture is a great idea!
dianes
Posts: 5
Joined: Fri Aug 26, 2005 2:53 pm
Location: Fort Collins, CO

Re: Help with disaster fire

Post by dianes »

Dang spellcheck. Shelf!
Ed Cantarella
Posts: 155
Joined: Mon Feb 26, 2018 3:49 pm
Location: Highland, Michigan, USA

Re: Help with disaster fire

Post by Ed Cantarella »

dianes wrote:Dang spellcheck. Shelf!
At least it wasn't elf. :)

BOT - what a drag. :-q(-_-)p All the suggestions above.
Attachments
eecab89039ec15b77cc483c32348d67c.jpg
HER last words were, "I'm melting, melting . . . " Dissenting opinions generally welcome for comic relief or personal edification. Sometimes both.
Post Reply