I am ball milling some glass down to use as a frit for fusing and I have a question. I have had a problem with milkiness in my clear powder and I assume that it is because I have not been screening out the extremely fine particles out of powder that I have run through an 80 mesh screen. Does anyone know what the particle size is for most of the commercial frits that are called "powder"?
-
Brad Walker
- Site Admin
- Posts: 1542
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: Powder Frit
Bullseye's powder is 0.2mm and smaller, which is what goes through an 80 mesh screen.
-
Terry Gallentine
- Posts: 195
- Joined: Mon Jul 19, 2004 2:08 pm
- Location: River Falls, WI
- Contact:
Re: Powder Frit
Thanks Brad. Do you have any ideas of how to get rid of the super fine particles?
-
Brad Walker
- Site Admin
- Posts: 1542
- Joined: Fri Mar 07, 2003 9:33 pm
- Location: North Carolina, USA
- Contact:
Re: Powder Frit
My first thought was what was causing them. Wonder if you're pulverizing more than Bullseye does.
As for getting rid of them, I think I would try rinsing the frit before you separate it into sizes.
Alternatively, get a finer mesh screen and try sifting them out. I know that Thompson Enamel will make different size screens.
As for getting rid of them, I think I would try rinsing the frit before you separate it into sizes.
Alternatively, get a finer mesh screen and try sifting them out. I know that Thompson Enamel will make different size screens.
-
Terry Gallentine
- Posts: 195
- Joined: Mon Jul 19, 2004 2:08 pm
- Location: River Falls, WI
- Contact:
Re: Powder Frit
It was my first attempt at ball milling some Easy Melt cullet from Wissmach and I probably did pulverize it too much. I was used to using scrap that I had to quench and stamp to make a gravel before I milled it and that took quite a while to mill down. I will try less time in the mill. I will probably try a wash and rinse of the frit to see if that eliminates most of the super fine particles.