Having never used a ceramic mold,  a couple questions:
3 or 4 coats of kiln wash?
prefire to ??
how long before needing to kiln wash again
do you sand off when needed or can you actually rinse of kiln wash with water?
will most glass slump at app 1200 - 1250?
one more question,  how the heck do you vacuum the kiln shelf without scratching it?
thanks,  archie
			
			
									
						
										
						first time using ceramic molds
Moderators: Brad Walker, Tony Smith
Re: first time using ceramic molds
archie wrote:Having never used a ceramic mold, a couple questions:
3 or 4 coats of kiln wash?
Or more. Make sure you can't see the colour of the mold through your kiln wash, that'll be enough.
prefire to ??
Pick a number. I fire high, others air dry.
how long before needing to kiln wash again
On a mold, firing low, sometimes a very long time. If the wash is chipping or spalling, redo it.
do you sand off when needed or can you actually rinse of kiln wash with water?
Depends on the wash, and the mix. I scrape and sand.
will most glass slump at app 1200 - 1250?
Yes.
one more question, how the heck do you vacuum the kiln shelf without scratching it?
Use the brush thingy accessory.
thanks, archie
My memory is so good, I can't remember the last time I forgot something . . .
			
						Re: first time using ceramic molds
500 degrees, 10 minutesarchie wrote: prefire to ??
do you sand off when needed or can you actually rinse of kiln wash with water?
I hand rub/sand very lightly. I have never removed all the old wash from my molds and have been firing in some of them for 17 years with no probs. Usually I just slap a new coat on if I have fired too high (above 1275) or accidentally chipped the wash off.
Brenda Griffith
Siyeh Studio
\^^^^^^:/_ When you are up to your ass in ALLIGATORS It's hard
\\^^^\\ to remember that the original task was to drain the swamp!
Re: first time using ceramic molds
Brenda 
I'm glad to see that I not the only one that doesn't take the wash off my molds. I hate to waste something that might still be good. I always buy my molds in greenware stage than bisque fire them myself. The other day I was using a bowl mold for the first time and instead of slumping I draped over it. The mold cracked. Have you ever had them crack on you and have you fixed them. I do have some clay slip but not sure if that will work.
Sandi
			
			
									
						
										
						I'm glad to see that I not the only one that doesn't take the wash off my molds. I hate to waste something that might still be good. I always buy my molds in greenware stage than bisque fire them myself. The other day I was using a bowl mold for the first time and instead of slumping I draped over it. The mold cracked. Have you ever had them crack on you and have you fixed them. I do have some clay slip but not sure if that will work.
Sandi
A lot of my molds came from a potter I was in an artist's co-op with in the late 80's. He made them in a rough red clay--definitely not porcelain... maybe terracotta or stoneware?--and didn't fire them all the way because he said the porosity would work better for multiple glass firings. *Shrug* I am barely successful at the physics of glass so I just said "ok". Anyway, one of my favorit bowls had a big piece of the edge chip off in a move and I glued it back together with a clay patch I got at a ceramic store in Austin. It seems to be holding up fine, but I don't know how it would work with a finer grained clay (or if the grain even matters).
			
			
									
						
							Brenda Griffith
Siyeh Studio http://www.siyehstudio.com
Glass Incarnate Daily Blog http://glassincarnate.blogspot.com/
A Beginner's Guide to Kiln-Formed Glass http://glassincarnate.com/thebook.html
			
						Siyeh Studio http://www.siyehstudio.com
Glass Incarnate Daily Blog http://glassincarnate.blogspot.com/
A Beginner's Guide to Kiln-Formed Glass http://glassincarnate.com/thebook.html
- 
				Cynthia
 
Re: first time using ceramic molds
No need to replace primer on molds unless you fire high for some reason or it gets scraped or worn away...Sandi wrote:Brenda
I'm glad to see that I not the only one that doesn't take the wash off my molds. I hate to waste something that might still be good. I always buy my molds in greenware stage than bisque fire them myself. The other day I was using a bowl mold for the first time and instead of slumping I draped over it. The mold cracked. Have you ever had them crack on you and have you fixed them. I do have some clay slip but not sure if that will work.
Sandi
It's a general rule of thumb that you shouldn't drape over clay because it does not contract as much as the glass will when cooling...which is most likely the reason your piece trapped the mold. (A shallow slope will work alright...like the sconce molds BE offers, but for the most part, draping over clay is dicey...) You can try using a defloculated slip to repair your mold. It will hold up, or not
- 
				Lauri Levanto
 - Posts: 270
 - Joined: Tue Mar 11, 2003 7:33 am
 - Location: Halikko, Finland
 
Priming bisque molds
I make ceramic moulds for my back relief castings.
I use to apply the first coat of shelf primer before
bisque firing. It seems to last severaql castings @850-880 C.
I mentioned this before, and got replies that kiln wash
"degrades" in those temperatures. My experience, however, is the opposite, and my guess for the reason is
that the kaolin matures in those temps. When in touch with
fluxes,it starts to melt into glass.
When fired separately, there is no fluxes. The kaolin
is sintered into the mould surface,
"locking in" the alumina. During subsequent firings
the alumina wears of and needs replacement at some point.
-lauri
			
			
									
						
										
						I use to apply the first coat of shelf primer before
bisque firing. It seems to last severaql castings @850-880 C.
I mentioned this before, and got replies that kiln wash
"degrades" in those temperatures. My experience, however, is the opposite, and my guess for the reason is
that the kaolin matures in those temps. When in touch with
fluxes,it starts to melt into glass.
When fired separately, there is no fluxes. The kaolin
is sintered into the mould surface,
"locking in" the alumina. During subsequent firings
the alumina wears of and needs replacement at some point.
-lauri