slumping bowls?????

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
bskirwin
Posts: 29
Joined: Sat Mar 29, 2003 9:41 am

slumping bowls?????

Post by bskirwin »

OK, what is the trick in making sure that your round blank sits evenly on the stainless steel bowl and slumps evenly in the mold.....??? I painstakenly try to place it on the rim of the mold evenly, and almost always end up with an uneven bowl. Arg!!!! Please give me any useful helpful hints. THanks. Barbara This is true for any size of bowl, from 4 inches in diameter to 16 inches in diameter.
Marty
Posts: 865
Joined: Mon Mar 10, 2003 3:58 pm
Location: Maine
Contact:

Post by Marty »

Is the kiln floor level? The mold, too? The blank is uniformly thick?
Try a bubble level on the blank to make sure it's level.
Try grinding a slight bevel on the rim to help it set in the mold.
Slump slowly.
Brock
Posts: 1519
Joined: Mon Mar 10, 2003 1:32 pm
Location: Vancouver, B.C.

Post by Brock »

Marty wrote:Is the kiln floor level? The mold, too? The blank is uniformly thick?
Try a bubble level on the blank to make sure it's level.
Try grinding a slight bevel on the rim to help it set in the mold.
Slump slowly.
Everything Marty said plus, DON'T SIT IT ON THE RIM.

Put your blank INSIDE the mold, down from the top any increment you desire.
This helps tremendously, in ensuring an even slump. Brock
My memory is so good, I can't remember the last time I forgot something . . .
Tony Serviente
Posts: 328
Joined: Thu May 29, 2003 11:48 am
Location: Ithaca,NY
Contact:

Post by Tony Serviente »

Without seeing your form I am going to guess it is steeply sided, and that will quite often give an uneven slump. Either a two firing approach will get it even, or putting a rim on it, and cutting it off after.
Post Reply