I did a small test piece using BE on the bottom... a very thin wafer centered on the BE... and BE clear on top. This was done on thin fiber paper. I used the 'sqeeze schedule'
300 - 1250 - 60
1000 - 1510 - 15
999 - 960 - 30
210 - 700 -
I STILL got bubbles!
Any suggestions would be greatly accepted.
Thanks,
Ross
More Bobble's Questions
Moderators: Brad Walker, Tony Smith
-
Jackie Beckman
- Posts: 475
- Joined: Sun Mar 09, 2003 5:01 pm
- Location: Arizona
- Contact:
-
Paul Tarlow
- Posts: 344
- Joined: Sun Mar 09, 2003 4:06 pm
- Location: Helios Kiln Glass Studio - Austin
- Contact:
Re: More Bobble's Questions
I'd fire twice. First to fuse the wafer smooth to the base. Then clear cap.Ross wrote:I did a small test piece using BE on the bottom... a very thin wafer centered on the BE... and BE clear on top. This was done on thin fiber paper. I used the 'sqeeze schedule'
300 - 1250 - 60
1000 - 1510 - 15
999 - 960 - 30
210 - 700 -
I STILL got bubbles!
Any suggestions would be greatly accepted.
Thanks,
Ross
Or - if the piece allows -- chad the outside of the clear cap higher than the wafer (and still squeeze).
Also, I'm having trouble understanding your schedule -- it looks like your first two segments overlap.
I use this schedule when I want to squeeze:
as fast as practical for the piece to 1150
1150 - 1250 @ 50 dph - 60 min hold
1250 to full fuse afap
down as appropriate for the piece
- Paul