Page 1 of 1

Drape question

Posted: Tue Jul 08, 2003 8:43 am
by deena
Does anyone have any sugesstions for creating a very narrow 6 inch long drape. Can i use a very small ss measuring cup on top of kiln furniture? I may have posted this question twice. Sorry

Thanks Deena

Posted: Tue Jul 08, 2003 2:50 pm
by Tony Serviente
Yes you can Deena. Make sure to kiln wash the SS well, and insure that the furniture it is resting on does not create an undercut, or else the glass may embrace the form, and not want to let go. Good luck.

Posted: Wed Jul 09, 2003 8:55 am
by deena
Thanks for your help. This board has made my learing curve much easier.
Would a longer soak time make the folds more pronounced?

I am looking for very tight folds.

Thanks
Deena

Posted: Wed Jul 09, 2003 11:43 am
by Stuart Clayman
YOu can also drape over a plumbing pipe that you can get at Home Despot. I put kiln wash on it and then also put thin fire under the piece.

Posted: Wed Jul 09, 2003 10:26 pm
by karla
Stuart:

What type of plumbing pipe are you speaking of - copper tubing?

Posted: Thu Jul 10, 2003 8:58 am
by rosanna gusler
not stewart but, regular black iron pipe. NOT galvanized. also steel bolts with a large fender washer and a nut under that. i put a piece of fiber on top. rosanna