Curious Glass enamel on float

This is the main board for discussing general techniques, tools, and processes for fusing, slumping, and related kiln-forming activities.

Moderators: Brad Walker, Tony Smith

Post Reply
Nelson Tan
Posts: 41
Joined: Sun Mar 09, 2003 9:23 pm
Location: Manila
Contact:

Curious Glass enamel on float

Post by Nelson Tan »

Just made two firings on float glass with opaque glass enamel

first one was fired to 1050 F
* the color is much like the color on the decal
* the design looks like "sticker" on the glass with design edges clearly
floating on top of float glass
* float glass still has sharp edges, corners are sharp too


second was fired to 1330 F
* the color shifted to transparent
* the design looks like it is embedded/fused on float glass
* float glass has rounded edges, corners are slightly rounded too

will try ceramic enamel next

nelson
Post Reply