Curious Glass enamel on float
Posted: Thu Aug 28, 2003 10:00 pm
Just made two firings on float glass with opaque glass enamel
first one was fired to 1050 F
* the color is much like the color on the decal
* the design looks like "sticker" on the glass with design edges clearly
floating on top of float glass
* float glass still has sharp edges, corners are sharp too
second was fired to 1330 F
* the color shifted to transparent
* the design looks like it is embedded/fused on float glass
* float glass has rounded edges, corners are slightly rounded too
will try ceramic enamel next
nelson
first one was fired to 1050 F
* the color is much like the color on the decal
* the design looks like "sticker" on the glass with design edges clearly
floating on top of float glass
* float glass still has sharp edges, corners are sharp too
second was fired to 1330 F
* the color shifted to transparent
* the design looks like it is embedded/fused on float glass
* float glass has rounded edges, corners are slightly rounded too
will try ceramic enamel next
nelson