combing problem
Moderators: Brad Walker, Tony Smith
-
Linda Hassur
- Posts: 44
- Joined: Sat Mar 15, 2003 10:40 pm
combing problem
I watched Patty Gray's demo of how she does her combing. I made combing tools according to her instruction. I'm having problems inthat they almost always stick on the lst pull and they bend as they aren't sturdy enough. I'm taking the glass to 1700. Any suggestions on tools used to pull the molten glass? Thanks Linda
-
Tony Smith
- Posts: 1037
- Joined: Sun Mar 09, 2003 5:59 pm
- Location: Massachusetts, USA
- Contact:
Patty's small combing tools are 316 stainless steel and 1/8" diameter. Her large combing tools are 3/16" diameter. If the diameter is too small, they will heat up quickly and stick to the glass. Increase the diameter of the stainless steel, and that should help. The 316 stainless rod is available from http://www.mcmaster.com
Tony
Tony
The tightrope between being strange and being creative is too narrow to walk without occasionally landing on both sides..." Scott Berkun