Page 1 of 1

Temperature help

Posted: Tue Sep 23, 2003 5:17 pm
by Rocky Gentry
I have an 8" X 8" fully fused 1/4" thick sand- blasted blank I need to
A) fire polish the ground edges of
B)fire polish the sand-blasted face of AND
C)slump

In what order do I execute those 3 steps, what temps would you use and how many firings will it take?

Any help is much appreciated. I have never fired sand-blasted glass before.

Can't really shoot 8-ball..... Rocky.

Posted: Tue Sep 23, 2003 5:26 pm
by charlie
operations are hottest to coolest.

if you want a completely glossy tile, in my kiln a firepolish would be 1300-1350. a & b would be done in one firing.

a slump would be at 1125-1250 depending upon size and distance to drop. the smaller the blank, the hotter it has to be. a 20" blank would be fully slumped at 1150 for 15 minutes for me, but an 8" would take 1250 for 20-30 minutes at least. i look in and see when it's slumped enough.

ymmv.

Posted: Tue Sep 23, 2003 6:46 pm
by rosanna gusler
no answers here but, good to hear from you! i miss your sense of humor on the board. well, i also watch south park. maybe that was not a compliment. lol. rosanna

Posted: Tue Sep 23, 2003 10:10 pm
by Rocky Gentry
I no longer have a sense of humor...Brad deleted it.

Posted: Tue Sep 23, 2003 10:16 pm
by Brock
Rocky Gentry wrote:I no longer have a sense of humor...Brad deleted it.
. . . you're gonna get mail . . .

Re: Temperature help

Posted: Wed Sep 24, 2003 5:08 am
by Brian and Jenny Blanthorn
Rocky Gentry wrote:I have an 8" X 8" fully fused 1/4" thick sand- blasted blank I need to
A) fire polish the ground edges of
B)fire polish the sand-blasted face of AND
C)slump

In what order do I execute those 3 steps, what temps would you use and how many firings will it take?

Any help is much appreciated. I have never fired sand-blasted glass before.

Can't really shoot 8-ball..... Rocky.
Yo Rocky

How is the polishing going ??

If U wanna silky fire polish U could do on the slump only

But U will pos pick up mould marks

I sand blast to 280

With a side fire kiln

I use Baffle n Go n Zap n Blastem tm

Use baffles 2 keep mould cool

But get top heat on glass from elements

Then fire after aneal temps on full

Dont open door peep

When fin crash cool

Brian

Re: Temperature help

Posted: Wed Sep 24, 2003 8:31 am
by Bert Weiss
Rocky Gentry wrote:I have an 8" X 8" fully fused 1/4" thick sand- blasted blank I need to
A) fire polish the ground edges of
B)fire polish the sand-blasted face of AND
C)slump

In what order do I execute those 3 steps, what temps would you use and how many firings will it take?

Any help is much appreciated. I have never fired sand-blasted glass before.

Can't really shoot 8-ball..... Rocky.
Rocky

You didn't mention what kind of glass. Any answers before that info are not too reliable.

Posted: Wed Sep 24, 2003 8:57 am
by Rocky Gentry
All Bullseye.