Page 1 of 1

Beginner's question

Posted: Sat Nov 01, 2003 1:15 pm
by Anna
Sorry about my English - I'm Russin sitting in Israel. :oops:
It was my very first "pure art" project, and it cracked! :cry:
One layer of gray cathedral Spectrum 96 70x30 cm with mosaic fish under it and clear "waves" above; large pieces of clear and white around (forming the thick layer of the "ice bank"); frits and small pieces of cold clear colours. I fired and annealed according to System96 instructions for
more than 20" and 3/8" thickness, 710C on top.
It has a long crack with the smooth edges going from the thick layer to the center. I tried to repair it by putting on pieces of clear glass and firing once again; it cracked second time near the first crack. Need a photo?
I need an advice of your years of experience!!!!!!!!!!

Re: Beginner's question

Posted: Sat Nov 01, 2003 3:25 pm
by Brian and Jenny Blanthorn
Anna wrote:Sorry about my English - I'm Russin sitting in Israel. :oops:
It was my very first "pure art" project, and it cracked! :cry:
One layer of gray cathedral Spectrum 96 70x30 cm with mosaic fish under it and clear "waves" above; large pieces of clear and white around (forming the thick layer of the "ice bank"); frits and small pieces of cold clear colours. I fired and annealed according to System96 instructions for
more than 20" and 3/8" thickness, 710C on top.
It has a long crack with the smooth edges going from the thick layer to the center. I tried to repair it by putting on pieces of clear glass and firing once again; it cracked second time near the first crack. Need a photo?
I need an advice of your years of experience!!!!!!!!!!
Russian in Israel

We very international here but is great

I am not very experianced still learning my self

But

If U got no mould ie undercuts

Then could B the surface undulations need more anealing

Thick thin realy needs more

One common first timer's thing is after aneal cooling 2 quick

Pic would help 4 the experts oppinion

But U will need 2 get used 2 things breaking / going wrong

But thats where the secret stuff is

U just gotta look

Another thing U realy need 2 do compatability test on all glass

Brian

Posted: Sat Nov 01, 2003 3:40 pm
by Tony Serviente
Brian is right about cooling big things down more slowly, and taking them out cooler than thin things. With all the right annealing schedules, and perfectly compatible glass, if you cool it too quickly it will crack. Pieces that go from thick to thin are particularly susceptible, due to the inherent unequal heat transfer rates within the piece. Wait to take it out till it is within 20 degrees or less of room temperature.

Posted: Sat Nov 01, 2003 5:44 pm
by Brucifer
Anna,

You said "It has a long crack with the smooth edges going from the thick layer to the center", does that mean your crack has smooth edges on it? Were you doing a tack fuse? I'm taking that the 710C is equalling 1310F. If the edges of the crack are melted over, you might of heated the piece too fast.

Bruce

Posted: Sat Nov 01, 2003 8:08 pm
by Barbara Muth
If the edges of the crak are smooth, then you cracked while heating up. With all the layers and varying levels of glass you probably need to heat up more slowly than the Spectrum schedule suggests. Another possibility could be incompatibility of some of your glass. Is it all system 96 glass? Any chance you used even a little something that was not system 96?

If you gave us more details about the glass and the schedule we could better help you. Posting a picture would help too.

Barbara

Posted: Sun Nov 02, 2003 3:37 pm
by Anna
Thanks!
It is in the kiln now - the third time.
Anna

Posted: Mon Nov 03, 2003 12:17 am
by steve_hiskey
if you get a crack in the same place again, my guess is that you have a piece of different COE glass.

I broke six bowls in a row one time before I realized that the scrap glass I was using to slump with from one glassblowing shop was COE90 and the other was COE 96.

(and I felt like and idiot afterwards)...

Steve